Method for suppressing formation of stacking faults, structure manufactured by method, and method for evaluating process-deteriorated layers
By removing the processing deterioration layer on the semiconductor substrate and performing etching and crystal growth processes, the problem of stacking fault formation is solved, the growth of low-density stacking faults on the semiconductor substrate is achieved, and the reliability of the semiconductor device and the substrate are improved. Surface flatness.
Patent Information
- Application Number
- CN202280092520.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-24
- Filing Date
- 2022-12-28
- Publication Date
- 2024-10-11
AI Technical Summary
The existing technology is difficult to effectively suppress stacking faults formed during epitaxial growth on semiconductor substrates, leading to the problem of abnormal voltage of power devices.
By removing the processing-degraded layer of the semiconductor substrate, using an etching process and a crystal growth process, the stacking fault density is measured to evaluate and suppress its formation.
It significantly reduces the density of stacking faults during epitaxial growth on semiconductor substrates, improves the reliability of semiconductor devices, and ensures substrate surface planarization and high-quality crystal growth.
Smart Images

Figure CN118765340A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for suppressing the formation of stacking faults, a structure produced by the method, and a method for evaluating a processing-deteriorated layer. Background Art
[0002] Generally, semiconductor substrates are manufactured by slicing semiconductor material ingots. On the surface of the sliced semiconductor substrate, there is a surface layer (hereinafter referred to as a processing-degraded layer) with crystal distortion and cracks introduced during slicing. In order not to reduce the yield in the device manufacturing process, it is necessary to flatten the substrate surface while removing the processing-degraded layer.
[0003] Various methods have been developed to remove and flatten the process-degraded layer according to the physical properties of semiconductor materials. For example, in silicon carbide (SiC), which is a compound semiconductor, multi-step mechanical grinding and polishing are performed to reduce the process-degraded layer and flatten the substrate surface.
[0004] Patent document 1 records the steps of a rough grinding process using abrasives such as diamond, a fine grinding process using abrasives smaller than those used in the rough grinding process, and a chemical mechanical polishing process (CMP) that simultaneously utilizes the mechanical action of a polishing pad and the chemical action of a polishing liquid to perform polishing, thereby reducing the processing deteriorated layer and flattening the substrate surface.
[0005] Prior art documents
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-5702 Summary of the invention
[0008] Problems to be solved by the present invention
[0009] In order to improve the reliability of semiconductor devices, it is desirable that various crystal defects and stacking faults (SF) present in an epitaxial layer grown on a semiconductor substrate have a low density. In particular, stacking faults are considered to be the cause of voltage anomalies in power devices, and it is desirable to form an epitaxial layer with fewer stacking faults.
[0010] The problem to be solved by the present invention is to provide a new technology capable of inhibiting the formation of stacking faults.
[0011] Furthermore, the problem to be solved by the present invention is to provide a new technology capable of suppressing stacking faults formed during epitaxial growth on a semiconductor substrate.
[0012] Solutions to the problem
[0013] The present invention for solving the above-mentioned problems provides a method for suppressing the formation of stacking faults, the method comprising: a process of removing a process-degraded layer of a semiconductor substrate; and a crystal growth process of growing crystals on a surface from which the process-degraded layer has been removed.
[0014] In a preferred embodiment of the present invention, the process for removing the machine-degraded layer is a process for removing the machine-degraded layer introduced by mechanical processing.
[0015] In a preferred embodiment of the present invention, the process of removing the machine-degraded layer is a process of etching the semiconductor substrate.
[0016] In a preferred embodiment of the present invention, the process of removing the processed degraded layer is a process of removing 1.5 μm or more from the surface of the semiconductor substrate.
[0017] In a preferred embodiment of the present invention, the process of removing the processed degraded layer is a process of removing 6.0 μm or more from the surface of the semiconductor substrate.
[0018] In a preferred form of the invention, the semiconductor substrate is silicon carbide.
[0019] The present invention provides a method for evaluating a process-deteriorated layer. That is, the present invention, which solves the above-mentioned problem, provides a method for evaluating a process-deteriorated layer, the method comprising: evaluating the process-deteriorated layer of the semiconductor substrate based on stacking faults formed during epitaxial growth on the semiconductor substrate.
[0020] In a preferred embodiment of the present invention, the evaluation process includes: an etching process for etching the processing-deteriorated layer of the semiconductor substrate; a crystal growth process for performing crystal growth on the surface of the etched processing-deteriorated layer; and a measurement process for measuring the density of stacking faults formed during the growth process in the crystal growth process.
[0021] In a preferred embodiment of the present invention, the evaluation process is a process of performing a plurality of measurements while varying the etching depth.
[0022] In a preferred form of the present invention, the etching process includes: a first etching process of etching to a first etching depth and a second etching process of etching to a second etching depth.
[0023] Effects of the Invention
[0024] According to the disclosed technology, a new technology for suppressing the formation of stacking faults can be provided.
[0025] Furthermore, according to the disclosed technology, a new technology capable of suppressing stacking faults formed during epitaxial growth on a semiconductor substrate can be provided.
[0026] Other objects, features and advantages will become apparent when the following detailed description is read in conjunction with the accompanying drawings and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 1 is an explanatory diagram showing a method of suppressing the formation of stacking faults according to the present invention.
[0028] Figure 2 It is an explanatory diagram showing a conventional method.
[0029] Figure 3 It is an explanatory diagram showing the etching process of the Example and the comparative example.
[0030] Figure 4 It is an explanatory diagram showing the crystal growth process of Examples and Comparative Examples.
[0031] Figure 5 Graphs showing the relationship between the stacking fault IGSF formed during the growth process and the etching depth ED in Examples and Comparative Examples. DETAILED DESCRIPTION
[0032] Hereinafter, preferred embodiments of a method for suppressing the formation of stacking faults, a structure manufactured by the method, and a method for evaluating a processed deteriorated layer according to the present invention will be described in detail with reference to the accompanying drawings. The technical scope of the present invention is not limited to the embodiments shown in the accompanying drawings, and may be appropriately modified within the scope of the claims. In addition, in this specification, in the notation of the Miller index, "-" represents a horizontal line attached to the index immediately following it, and appending "-" in front of the index represents a negative index. In addition, in the description and drawings of the following embodiments, the same components are represented by the same figure marks, and repeated descriptions will be omitted.
[0033] 《Method for inhibiting the formation of stacking faults》
[0034] like Figure 1 As shown, the method for suppressing the formation of stacking faults according to the present invention includes: a process S10 of removing the process-degraded layer 11 of the semiconductor substrate 10; and a crystal growth process S20 of crystal-growing the growth layer 20 on the surface from which the process-degraded layer 11 has been removed.
[0035] The present invention can suppress the formation of an internal growth stacking fault (IGSF) formed during the growth process by the process-degraded layer removal process S10 including removing the process-degraded layer 11. That is, it is considered that the stacking fault IGSF formed during the growth process is caused by the process-degraded layer 11 remaining on the surface of the semiconductor substrate 10.
[0036] Figure 21 is a conceptual diagram when the crystal growth process S20 is performed on the surface of the semiconductor substrate 10 where the process-degraded layer 11 remains. Figure 2 It is shown how stacking faults IGSF are generated in the growth layer 20 from the interface between the semiconductor substrate 10 and the growth layer 20 during the growth process when the process-degenerated layer 11 remains.
[0037] In addition, the term "process-degraded layer" in this specification refers to a layer introduced by mechanical processing on the surface of the semiconductor substrate 10. In addition, in order to determine whether the "process-degraded layer" has been removed, epitaxial growth is performed on the semiconductor substrate 10 from which the process-degraded layer 11 has been removed, and the stacking faults IGSF formed in the growth layer 20 during the growth process are observed and evaluated for confirmation.
[0038] Of course, any commonly used material can be used as the material of the semiconductor substrate 10. Semiconductor materials are, for example, known IV group materials such as silicon (Si), germanium (Ge), and diamond (C). In addition, the material of the semiconductor substrate 10 is, for example, a known IV-IV group compound semiconductor material such as silicon carbide (SiC). In addition, the material of the semiconductor substrate 10 is a known II-VI group compound semiconductor material such as zinc oxide (ZnO), zinc sulfide (ZnS), zinc selenide (ZnSe), cadmium sulfide (CdS), and cadmium telluride (CdTe). In addition, the material of the semiconductor substrate 10 is, for example, a known III-V group compound semiconductor material such as boron nitride (BN), gallium arsenide (GaAs), gallium nitride (GaN), aluminum nitride (AlN), indium nitride (InN), gallium phosphide (GaP), indium phosphide (InP), and indium antimonide (InSb). In addition, the material of the semiconductor substrate 10 is, for example, a known oxide semiconductor material such as aluminum oxide (Al2O3) and gallium oxide (Ga2O3). Furthermore, the semiconductor substrate 10 may have a structure to which known additive atoms used according to the material thereof are appropriately added.
[0039] In addition, as a preferred material for the semiconductor substrate 10 used in the present invention, the above-mentioned compound semiconductors can be cited. For example, compound semiconductors such as single crystal SiC are hard and brittle materials and are classified as extremely difficult to process. The method according to the present invention can suppress the formation of stacking faults IGSF formed during the growth process by removing the processing-degraded layer 11 before growing the compound semiconductor growth layer 20.
[0040] <Processing Deteriorated Layer Removal Process S10>
[0041] Next, the machining-deteriorated layer removal process S10 according to the present invention will be described in detail.
[0042] The process S10 is a process for removing the process-deteriorated layer 11 introduced on the surface of the semiconductor substrate 10 by a process involving mechanical processing such as slicing, rough grinding, fine grinding, chemical mechanical polishing, etc. In other words, it is a process for removing the process-deteriorated layer 11 of the semiconductor substrate 10 and exposing the main layer 12.
[0043] By performing the process S10 of removing the processing-deteriorated layer on the semiconductor substrate 10 after the chemical mechanical polishing process, the processing-deteriorated layer 11 causing the stacking faults IGSF formed during the growth process may be removed.
[0044] Thermal etching can be used as a method for removing the process-degraded layer 11. As thermal etching, for example, H2 etching, Si vapor pressure etching, sublimation etching, etc. can be used.
[0045] In the processing deteriorated layer removal process S10, the etching depth ED from the surface of the semiconductor substrate 10 increases or decreases according to the depth (thickness) of the processing deteriorated layer 11 introduced into the semiconductor substrate 10, but is preferably greater than 0.5μm, more preferably greater than 1.0μm, further preferably greater than 1.5μm, further preferably greater than 2.0μm, further preferably greater than 3.0μm, further preferably greater than 4.0μm, further preferably greater than 5.0μm, and further preferably greater than 6.0μm.
[0046] In the region where the process-degenerated layer 11 is present, the more the etching amount increases (i.e., the deeper the etching depth ED becomes), the more the formation of the stacking fault IGSF formed during the epitaxial growth process is suppressed. In addition, in a state where the process-degenerated layer 11 is removed and the main layer 12 is exposed, the formation of the stacking fault IGSF formed during the growth process is almost zero. Therefore, the depth of the process-degenerated layer 11 introduced into the semiconductor substrate 10 can be evaluated by determining the etching depth ED at which the formation of the stacking fault IGSF formed during the growth process is almost zero.
[0047] <Crystal Growth Process S20>
[0048] Next, the crystal growth process S20 according to the present invention will be explained in detail.
[0049] The crystal growth process S20 is a process of forming a growth layer 20 by performing epitaxial growth on the surface of the semiconductor substrate 10 from which the altered layer 11 has been removed in the altered layer removal process S10 .
[0050] As a method for forming the growth layer 20 , for example, a known film forming method such as a physical vapor deposition method (PVD method) or a chemical vapor deposition method (CVD method) can be used.
[0051] The density of stacking faults IGSF formed in the growth layer 20 during the growth process is preferably 3.0 pieces / cm 2 Below, more preferably 2.0 pieces / cm 2 Below, more preferably 1.0 piece / cm 2 Below, more preferably almost 0 pieces / cm 2 .
[0052] The method for measuring the presence or absence and density of stacking faults IGSF formed during the growth process can adopt the following known methods for detecting stacking faults SF: photoluminescence (PL), transmission or reflection X-ray topography (XRT), dislocation evaluation by chemical etching, and Raman spectroscopy analysis, etc.
[0053] According to the method of suppressing the formation of stacking faults of the present invention, the stacking faults IGSF formed during the epitaxial growth process can be suppressed by the process of removing the process-degraded layer 11 in the process of removing the process-degraded layer S10 .
[0054] According to the method for suppressing the formation of stacking faults of the present embodiment, the process S10 is a process of removing the process-degraded layer 11 introduced by performing mechanical processing. In addition, the process S10 is a process of removing the process-degraded layer 11 introduced by performing a chemical mechanical polishing process.
[0055] By the method for suppressing the formation of stacking faults according to the embodiment, a semiconductor substrate having a low density of stacking faults IGSF formed during the growth process can be manufactured. In addition, by the method for suppressing the formation of stacking faults according to the embodiment, a semiconductor device having a low density of stacking faults IGSF formed during the growth process can be manufactured. In addition, the semiconductor device includes, for example, a Schottky barrier diode, a junction barrier Schottky diode, a thyristor, a bipolar junction transistor, and a PiN diode.
[0056] <<Method for evaluating machining-degraded layers>>
[0057] The method for evaluating a process-degraded layer according to the present invention includes an evaluation process for evaluating a process-degraded layer 11 of a semiconductor substrate 10 based on stacking faults IGSF formed during the growth of the semiconductor substrate 10. In addition, components substantially the same as those shown in the previous embodiment are given the same reference numerals to simplify the description.
[0058] When the process-degenerated layer 11 exists at the interface between the semiconductor substrate 10 and the growth layer 20, a stacking fault IGSF (see FIG. 1 ) formed during the growth process due to the process-degenerated layer 11 occurs in the growth layer 20. Figure 2 ).
[0059] Therefore, by forming the growth layer 20 on the semiconductor substrate 10 to be evaluated and evaluating the stacking faults IGSF formed during the growth process, it is possible to evaluate whether the process-affected layer 11 remains in the semiconductor substrate 10 .
[0060] The evaluation process according to the present embodiment includes an etching process for etching the process-degraded layer 11 of the semiconductor substrate 10, a crystal growth process for growing crystals on the surface of the etching process-degraded layer 11, and a measurement process for measuring the density of stacking faults IGSF formed during the growth process in the crystal growth process.
[0061] The method for measuring the presence or absence and density of stacking faults IGSF formed during the growth process can adopt the following known methods for detecting stacking faults SF: photoluminescence (PL), transmission or reflection X-ray topography (XRT), dislocation evaluation by chemical etching, and Raman spectroscopy analysis, etc.
[0062] The evaluation process according to the embodiment includes a process of performing a plurality of measurements while changing the etching depth ED. That is, the semiconductor substrate 10 as the evaluation object is subjected to an etching process to obtain different etching depths ED, and then a crystal growth process and a measurement process are performed. In this way, by evaluating the correspondence between different etching depths ED and the density of stacking faults IGSF formed during the growth process, the depth of the process-degraded layer 11 remaining in the semiconductor substrate 10 as the evaluation object can be determined.
[0063] Example
[0064] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples. In addition, the present invention is not limited to the following contents.
[0065] The substrates used in the following examples and comparative examples were cut into a size of 25 mm × 10 mm from a 4H-SiC wafer tilted 4 degrees in the <11-20> direction after chemical mechanical polishing. In other words, the substrates used in the examples and comparative examples were cut from the same wafer that had been finished by CMP.
[0066] The apparatus used in the following examples and comparative examples is the apparatus described in International Publication No. 2021 / 025085, and includes a main body container 30, a high melting point container 40, and a heating furnace capable of accommodating the main body container 30 and the high melting point container 40 and heating to form a temperature gradient (see Figure 3 and Figure 4 ).
[0067] (Main container 30)
[0068] The main body container 300 may be configured as long as it can accommodate the semiconductor substrate 10 and generate vapor pressure in the internal space of the gas phase species containing the Si element and the gas phase species containing the C element during the heat treatment. For example, the main body container 30 is formed of a material containing SiC, preferably a material containing polycrystalline SiC. In addition, the main body container 30 is preferably in a form in which SiC is exposed on at least a portion of the inner surface of the container.
[0069] exist Figure 3 and 4 In the illustrated embodiment, the entire main body container 30 is made of polycrystalline SiC. By heating the main body container 30 made of such a material, vapor pressure of the gas species containing Si element and the gas species containing C element can be generated in the main body container 30.
[0070] That is, it is preferred that the environment in the main body container 30 after the heat treatment is a vapor pressure environment of a mixed system of gas phase seeds containing Si element and gas phase seeds containing C element. Examples of gas phase species containing Si element include Si, Si2, Si3, Si2C, SiC2, SiC, etc. In addition, examples of gas phase seeds containing C element include Si2C, SiC2, SiC, C, etc. That is, a state in which SiC-based gas exists in the main body container 30.
[0071] In addition, any structure may be adopted as long as the vapor pressure of the gaseous species containing Si element and the gaseous species containing C element is generated in the internal space during the heat treatment of the main body container 30. For example, a structure in which the polycrystalline SiC is exposed on a part of the inner surface, a structure in which the polycrystalline SiC is separately arranged inside the main body container 30, etc. may be shown.
[0072] like Figure 3 and 4 As shown, the main body container 30 is an assembly container, which includes an upper container 31 and a lower container 32 that can be assembled with each other. A small gap 33 is formed at the fitting portion of the upper container 31 and the lower container 32, and the main body container 30 is configured to be able to be exhausted (vacuumed) through the gap 33. That is, the interior of the main body container 30 becomes a quasi-enclosed space when exhausting.
[0073] The term "semi-enclosed space" used herein refers to a space in which the interior of the container can be evacuated but at least a portion of the steam generated in the container can be restricted. The semi-enclosed space can be formed in the container.
[0074] Figure 31 is an explanatory diagram showing an arrangement when etching a semiconductor substrate 10, which is a process of transporting Si atoms and C atoms on the semiconductor substrate 10 side to the main body container 30 side using the temperature difference set between the semiconductor substrate 10 and the main body container 30 as a driving force. That is, due to the temperature gradient formed by the heating furnace, at least a portion of the main body container 30 (for example, the bottom surface of the lower container 32) becomes lower in temperature than the semiconductor substrate 10, thereby generating a driving force for transporting Si atoms and C atoms on the semiconductor substrate 10 side to the main body container 30 side.
[0075] More specifically, when comparing the temperature of the surface of the semiconductor substrate 10 to be etched and the temperature of the bottom surface of the lower container 32 facing the surface, heating is performed so that the temperature on the semiconductor substrate 10 side is higher, while the temperature on the semiconductor substrate 10 side is lower. In this way, by forming a space having a temperature difference between the semiconductor substrate 10 and the lower container 32 in the main body container 30, the Si atoms and C atoms on the semiconductor substrate 10 side can be transported to the lower container 32 using the temperature difference as a driving force. In addition, although not shown, a substrate holder for holding the semiconductor substrate 10 may be provided, or the temperature gradient of the heating furnace may be reversed.
[0076] Figure 4 1 is an explanatory diagram showing an arrangement for epitaxial growth on a semiconductor substrate 10, which is a process for transporting Si atoms and C atoms from the main body container 30 side to the semiconductor substrate 10 side using the temperature difference set between the main body container 30 and the semiconductor substrate 10 as a driving force. That is, due to the temperature gradient formed by the heating furnace, at least a portion of the main body container 30 (for example, the top surface of the upper container 31) becomes a higher temperature than the semiconductor substrate 10, thereby generating a driving force for transporting Si atoms and C atoms on the main body container 30 side to the semiconductor substrate 10 side.
[0077] More specifically, when comparing the temperature of the surface on the semiconductor substrate 10 where epitaxial growth is performed and the temperature of the top surface of the upper container 31 facing the surface, heating is performed so that the temperature on the semiconductor substrate 10 side is lower, while the temperature on the semiconductor substrate 10 side is lower. In this way, by forming a space having a temperature difference between the semiconductor substrate 10 and the upper container 31 in the main body container 30, Si atoms and C atoms in the upper container 31 can be transported to the semiconductor substrate 10 using the temperature difference as a driving force. In addition, although not shown, a substrate holder for holding the semiconductor substrate 10 may be provided, or the temperature gradient of the heating furnace may be reversed.
[0078] (High melting point container 40)
[0079] The high melting point container 40 is configured to contain a high melting point material, such as C as a general heat-resistant component, W, Re, Os, Ta, Mo as a high melting point metal, Ta9C8, HfC, TaC, NbC, ZrC, Ta2C, TiC, WC, MoC as carbides, HfN, TaN, BN, Ta2N, ZrN, TiN as carbides, HfB2, TaB2, ZrB2, NB2, TiB2 as borides, and polycrystalline SiC, etc.
[0080] Similar to the main body container 30, the high melting point container 40 is a fitting container including an upper container 41 and a lower container 42 that can fit together, and is configured to accommodate the main body container 30. A small gap 43 is formed at the fitting portion of the upper container 41 and the lower container 42, and it is configured to exhaust (evacuate) the inside of the high melting point container 40 through the gap 43. That is, the inside of the high melting point container 40 becomes a quasi-enclosed space when exhausting.
[0081] The high melting point container 40 has a Si vapor supply source 44 capable of supplying a vapor pressure of a gas phase seed containing Si element into the high melting point container 40. The Si vapor supply source 44 can be any structure as long as it generates Si vapor in the high melting point container 40 during heat treatment, and examples thereof include solid Si (Si particles such as single crystal Si wafers and Si powders) and Si compounds. For example, a layer made of a silicided high melting point material can be provided inside the high melting point container 40.
[0082] In addition to this, any structure may be used as long as the vapor pressure of the gaseous species containing the Si element is generated in the high melting point container 40 during the heat treatment.
[0083] <Example 1>
[0084] The (0001) plane (=Si plane) of the semiconductor substrate 10 was etched to an etching depth ED of 6.0 μm, and then crystal growth was performed to a growth amount of 14.0 μm. Thereafter, the stacking fault IGSF formed during the growth process was measured using the PL method.
[0085] (Etching process)
[0086] In the etching process according to Example 1, the cut semiconductor substrate 10 is placed in the main body container 30, and the main body container 30 is further placed in the high melting point container 40, and heated to 1800° C. by using a heating furnace, and the (0001) plane (=Si plane) of the semiconductor substrate 10 is etched by 6.0 μm (see Figure 3 ).
[0087] (Crystal Growth Process)
[0088] In the crystal growth process according to Example 1, the semiconductor substrate 10 subjected to the etching process is placed in the main body container 30, and the main body container 30 is further placed in the high melting point container 40, and heated to 1800° C. by using a heating furnace, and a 14.0 μm crystal is grown on the (0001) plane (=Si plane) of the semiconductor substrate 10 (see Figure 4 ).
[0089] (Measurement process)
[0090] In the measurement process according to Example 1, the semiconductor substrate 10 that has undergone the crystal growth process is measured by the PL method (incident light: 313 nm, detector: >750 nm). From the PL image of this Example 1, no stacking faults IGSF formed during the growth process are observed. Therefore, the density of the stacking faults IGSF formed during the growth process is 0 pieces / cm 2 , and it is considered that the process-degraded layer 11 of the semiconductor substrate 10 has been removed.
[0091] <Comparative Example 1>
[0092] The (0001) plane (=Si plane) of the semiconductor substrate 10 cut out from the same wafer as in Example 1 was etched to an etching depth ED of 1.3 μm, and then crystal growth was performed to a growth amount of 14.0 μm. Thereafter, the stacking fault IGSF formed during the growth process was measured using the PL method.
[0093] (Etching process)
[0094] In the etching process of Comparative Example 1, the cut semiconductor substrate 10 is placed in a main container 30, and the main container 30 is placed in a high melting point container 40, and is heated to 1700°C using a heating furnace, so that the (0001) surface (=Si surface) of the semiconductor substrate 10 is etched by 1.3μm.
[0095] (Crystal Growth Process)
[0096] In the crystal growth process according to Comparative Example 1, crystal growth was performed under the same conditions as in Example 1.
[0097] (Measurement process)
[0098] In the measurement process of Comparative Example 1, the measurement was performed by the PL method under the same conditions as in Example 1. The density of stacking faults IGSF formed during the growth process obtained from the PL image of Comparative Example 1 was 2.5 pieces / cm 2 .
[0099] <Comparative Example 2>
[0100] The (0001) plane (=Si plane) of the semiconductor substrate 10 cut out from the same wafer as in Example 1 was etched to an etching depth ED of 0.6 μm, and then crystal growth was performed to a growth amount of 14.0 μm. Thereafter, the stacking fault IGSF formed during the growth process was measured using the PL method.
[0101] (Etching process)
[0102] In the etching process of Comparative Example 2, the cut semiconductor substrate 10 is placed in a main container 30, and the main container 30 is placed in a high melting point container 40, and is heated to 1700°C using a heating furnace, so that the (0001) surface (=Si surface) of the semiconductor substrate 10 is etched by 0.6μm.
[0103] (Crystal Growth Process)
[0104] In the crystal growth process according to Comparative Example 2, crystal growth was performed under the same conditions as in Example 1.
[0105] (Measurement process)
[0106] In the measurement process of Comparative Example 2, the measurement was performed by the PL method under the same conditions as in Example 1. The density of stacking faults IGSF formed during the growth process obtained from the PL image of Comparative Example 2 was 13.5 pieces / cm 2 .
[0107] <Comparative Example 3>
[0108] Crystal growth was performed on the (0001) plane (=Si plane) of the semiconductor substrate 10 cut out from the same wafer as in Example 1, and the crystal growth was performed so that the growth amount was 14.0 μm. That is, crystal growth was performed on the surface after CMP without etching. Thereafter, the stacking fault IGSF formed during the growth process was measured using the PL method.
[0109] (Crystal Growth Process)
[0110] In the crystal growth process according to Comparative Example 3, crystal growth was performed under the same conditions as in Example 1.
[0111] (Measurement process)
[0112] In the measurement process of Comparative Example 3, the measurement was performed by the PL method under the same conditions as in Example 1. The density of stacking faults IGSF formed during the growth process obtained from the PL image of Comparative Example 3 was 32.0 pieces / cm 2 .
[0113] Figure 5Graphs showing the relationship between the stacking fault IGSF formed during the growth process and the etching depth ED in Examples and Comparative Examples.
[0114] like Figure 5 As shown in FIG. 1 , the density of stacking faults IGSF formed during the growth process in the semiconductor substrate 10 subjected to the crystal growth process without the etching process is 32 pieces / cm 2 On the other hand, the density of stacking faults IGSF formed during the growth process in the semiconductor substrate 10 subjected to the crystal growth process after the etching process was 13.5 pieces / cm 2 , 2.5 / cm 2 and 0 / cm 2 ,Obviously, with the increasing etching depth, the density of the stacking faults IGSFs formed during the growth process decreases.
[0115] In Example 1, the density of stacking faults IGSF formed during the growth process is 0 / cm 2 However, it is considered that etching to a depth ED of 6.0 μm is excessive.
[0116] When compared with the results of Example 1 and Comparative Example 1, it can be estimated that if the etching depth ED is 1.5 μm or more, a growth layer 20 in which no stacking fault IGSF is formed during the growth process can be obtained.
[0117] According to the embodiment and the comparative example, the process S10 may be a process of removing 1.5 μm or more from the surface of the semiconductor substrate 10. In addition, the process S10 may be a process of removing 6.0 μm or more from the surface of the semiconductor substrate 10.
[0118] Furthermore, the embodiments and comparative examples can be understood as a method for evaluating a process-degraded layer, which includes: an evaluation process for evaluating a process-degraded layer 11 of a semiconductor substrate 10 based on stacking faults IGSF formed during epitaxial growth on the semiconductor substrate 10 .
[0119] The evaluation process includes an etching process of etching the process-degraded layer 11 of the semiconductor substrate 10, a crystal growth process of growing crystals on the etched surface of the process-degraded layer 11, and a measurement process of measuring the density of stacking faults IGSF formed during growth in the crystal growth process.
[0120] In the evaluation process, the depth of the process-deteriorated layer 11 introduced into the semiconductor substrate 10 can be evaluated by performing a plurality of measurements while changing the etching depth ED. Specifically, the depth of the process-deteriorated layer 11 can be estimated by a first etching process including etching to a first etching depth and a second etching process including etching to a second etching depth.
[0121] That is, the depth of the process-degraded layer 11 introduced into the semiconductor substrate 10 (wafer used this time) can be estimated to be about 1.5 μm based on the results of Example 1 and Comparative Example 1. In addition, the depth of the process-degraded layer 11 varies depending on the surface finish and quality of the wafer.
[0122] Explanation of symbols
[0123] 10Semiconductor substrate
[0124] 11 Processing metamorphic layer
[0125] 12 Main layer
[0126] 20 Growth Layer
[0127] 30 Main container
[0128] 31 containers
[0129] 32 containers
[0130] 33 Gap
[0131] 40 High Melting Point Container
[0132] 41 Upper container
[0133] 42 lower container
[0134] 43 Gap
[0135] 44Si steam supply source
[0136] S10 machining metamorphic layer removal process
[0137] S20 Crystal Growth Process
[0138] ED etching depth
[0139] Stacking faults formed during the growth of IGSF.
Claims
1. A method for inhibiting the formation of stacking faults, the method comprising: A process for removing a processing-deteriorated layer of a semiconductor substrate; as well as A crystal growth process is performed to grow crystals on the surface from which the machining-affected layer has been removed.
2. The method according to claim 1, wherein: The process of removing the machine-degraded layer is a process of removing the machine-degraded layer introduced by machining.
3. The method according to claim 1 or 2, wherein: The process of removing the machine-degraded layer is a process of etching the semiconductor substrate.
4. The method according to any one of claims 1 to 3, wherein: The process of removing the processed degraded layer is a process of removing 1.5 μm or more from the surface of the semiconductor substrate.
5. The method according to any one of claims 1 to 3, wherein: The process of removing the damaged layer is a process of removing 6.0 μm or more from the surface of the semiconductor substrate.
6. The method according to any one of claims 1 to 5, wherein: The semiconductor substrate is silicon carbide.
7. A semiconductor substrate manufactured by the method according to claims 1 to 6.
8. A semiconductor device manufactured using the semiconductor substrate according to claim 7.
9. A method for evaluating a processing-deteriorated layer, the method comprising: An evaluation process for evaluating a processing-degraded layer of a semiconductor substrate based on stacking faults formed during epitaxial growth on the semiconductor substrate.
10. The method according to claim 9, wherein: The evaluation process includes: An etching process for etching a processed deteriorated layer of a semiconductor substrate; A crystal growth process for performing crystal growth on the surface of the etched processed altered layer; A measurement process for measuring the density of stacking faults formed during growth in the crystal growth process.
11. The method according to claim 10, wherein: The evaluation process is a process of performing a plurality of measurements while changing the etching depth.
12. The method according to claim 10, wherein: The etching process includes a first etching process of etching to a first etching depth and a second etching process of etching to a second etching depth.