Production process of wood fiber culture medium block

Through wood fiber shaving, hot grinding and hot pressing processes, the problems of long water absorption time and poor fertilizer retention performance of soilless cultivation matrix blocks are solved, and a matrix block suitable for seedlings and cultivation is produced, which has low cost, good degradability and Features of high expansion ratio.

CN118765749AInactive Publication Date: 2024-10-15HENAN QINGDA FUNONG BIOTECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411096058.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-15
Filing Date
2024-08-12
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing soilless cultivation matrix block production process has problems such as long water absorption time, hardness after water absorption, small number of gaps, and poor water absorption and fertilizer retention performance, making it unsuitable for plant seedlings and cultivation.

Method used

A wood fiber cultivation matrix block production process is adopted, including wood chipping, thermal grinding, drying, mechanical vacuum paving, pre-pressing, hot pressing and other steps. The hot pressing temperature and pressure are controlled to form a high expansion multiple, softness and water retention properties. Good matrix block.

Benefits of technology

The substrate block produced has low cost, good degradability, short water absorption time, softness after water absorption, many voids, and good fertilizer retention performance. It is suitable for plant seedlings and cultivation, and is easy to transport.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987961320000081
    Figure BDA0004987961320000081
  • Figure BDA0004987961320000091
    Figure BDA0004987961320000091
  • Figure BDA0004987961320000101
    Figure BDA0004987961320000101
Patent Text Reader

Abstract

The invention discloses a wood fiber culture medium block production process. The wood fiber culture medium block production process comprises the following steps that S1, wood is made into wood chips through a chipping machine; s2, the wood chips are screened; s3, the screened wood chips are subjected to high-temperature cooking and mechanical separation, and fibers are obtained; s4, drying the fibers; s5, mechanical vacuum paving is carried out; s6, the soft plate blank is subjected to pre-pressing; s7, trimming, sawing and cutting are conducted on the pre-pressed and formed plate blank; s8, the fiber board blank is heated, pressure is applied, and the fiber board blank is subjected to compression molding; s9, cooling the fiberboard subjected to hot press molding; s10, sawing the fiberboard into shapes of seedling blocks, cultivating blocks, planting blocks and matrix strips, and processing planting holes in the upper parts of the fiberboard; the matrix block produced by the invention has the advantages of low cost, easiness in degradation and no secondary pollution; the fertilizer has good water absorption and fertilizer retention performance and is suitable for plant seedling culture and cultivation; the matrix block is high in expansion multiple when absorbing water to a saturated state, and is convenient to transport.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of soilless cultivation, in particular to a production process of a wood fiber cultivation matrix block. Background Art

[0002] In recent years, soilless cultivation has gradually emerged, and the soilless cultivation substrate is crucial to the growth of plants. Substrate cultivation is the most widely used soilless cultivation technology. The roots of plants are fixed in the substrate. The organic matter content, fertilizer retention capacity, water retention, air permeability, etc. of the substrate have an important influence on the growth of plants; Patent publication number CN1958718A discloses a composite soil-seeded wood fiber and its manufacturing method, which specifically discloses a method of using wood as a raw material to make wood chips by chipping, and then softening the wood chips in a hot mill and then grinding them into bundles of fibers with a hot grinding disc, and spraying an aqueous solution of a surfactant into the bundles of fibers to obtain a composite soil-seeded wood fiber. The wood fiber has good Water retention is used to repair landform planting areas with extremely serious soil loss. Since soilless cultivation requires the use of substrate blocks with a certain shape as carriers to cultivate plants (such as seedling blocks, cultivation blocks and planting blocks), it is necessary to hot-press wood fibers into substrate blocks. However, the substrate blocks produced by the existing hot-pressing process have the problems of taking a long time to absorb water to a saturated state, being inconvenient to use, being hard when absorbing water to a saturated state, having a small number of voids when absorbing water to a saturated state, and having poor water absorption and fertilizer retention performance, and are not suitable for plant seedling and cultivation use; the expansion multiples of the substrate blocks when absorbing water to a saturated state are low, making them inconvenient to transport, and the like. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the existing defects and provide a production process for wood fiber cultivation substrate blocks. The produced substrate blocks are low in cost, good in degradability, and will not cause secondary pollution to the environment; the time required for absorbing water to a saturated state is short, and the use is convenient; the substrate blocks are relatively soft when absorbing water to a saturated state, the number of gaps when absorbing water to a saturated state is large, the water absorption and fertilizer retention performance is good, and the substrate blocks are suitable for plant seedling and cultivation; the substrate blocks have a high expansion multiple when absorbing water to a saturated state, and the substrate blocks are in a compressed state before use, which is convenient for transportation, and can effectively solve the problems in the background technology.

[0004] To achieve the above object, the present invention provides the following technical solution: a process for producing a wood fiber cultivation matrix block, comprising the following steps:

[0005] S1. Chipping: The wood is processed into wood chips by a chipper;

[0006] S2. Screening: Screen the wood chips produced by the chipper and select the wood chips that meet the size requirements for the next process;

[0007] S3, hot grinding: the screened wood chips are steamed at high temperature and mechanically separated to obtain fibers;

[0008] S4, drying: drying the fiber by controlling the ambient temperature so that the moisture content of the fiber after drying is 10% to 15%;

[0009] S5. Paving: mechanical vacuum paving;

[0010] S6, pre-pressing: pre-pressing the soft slab;

[0011] S7, slab sawing: trimming and sawing the pre-pressed slab;

[0012] S8, hot pressing: heating the fiber mat and applying pressure to densify the fluffy fiber mat, so as to press the fiber mat into shape; the hot pressing is divided into three stages: the first stage applies high pressure to the mat to shape its upper and lower surfaces, and the pressure is controlled between 1.8 and 2.3 MPa; the second stage makes the surface temperature of the mat transfer heat to the core, and the pressure is controlled between 0.9 and 1.2 MPa; the third stage is to solidify the mat as a whole and shape it into a fixed thickness, and the pressure is controlled between 1.8 and 2.1 MPa, and the temperature of the whole hot pressing process is controlled between 120℃ and 140℃;

[0013] S9, cooling: cooling the hot-pressed fiberboard;

[0014] S10. Sawing and processing according to different uses: sawing and cutting the fiberboard into the shapes of seedling blocks, cultivation blocks, planting blocks and substrate strips, and processing the planting holes on the upper parts thereof.

[0015] Furthermore, the cooking temperature of step S2 is 160°C to 180°C.

[0016] Furthermore, the average length of the fibers obtained by mechanical separation in step S2 is 1 to 3 cm.

[0017] Furthermore, after the hot grinding in step S3, a conditioner can be added according to planting needs.

[0018] Furthermore, the fiberboard formed by hot pressing in step S9 is cooled on a cooling panel turning machine.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: the production process of the wood fiber cultivation matrix block is low in cost and good in degradability because the cultivation matrix block is made of wood fiber and will not cause secondary pollution to the environment; the time required to absorb water to a saturated state is short, the matrix block is relatively soft when it absorbs water to a saturated state, the number of voids when it absorbs water to a saturated state is large, the water absorption and fertilizer retention performance is good, and the matrix block is suitable for plant seedling and cultivation; the matrix block has a high expansion multiple when it absorbs water to a saturated state, and the matrix block is in a compressed state before use, which is convenient for transportation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a diagram showing the changes of the matrix block produced by the matrix block production process of the present invention before and after water absorption;

[0021] Figure 2 A schematic diagram of the cross-sectional density distribution of a matrix block produced by the matrix block production process of the present invention;

[0022] Figure 3 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 1;

[0023] Figure 4 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 2;

[0024] Figure 5 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 3;

[0025] Figure 6 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 4;

[0026] Figure 7 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 5;

[0027] Figure 8 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 6;

[0028] Fig. 9 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 7;

[0029] Fig.10 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 8;

[0030] Fig.11 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 9;

[0031] Fig.12 A schematic diagram of the structure of a matrix block produced by the matrix block production process of Comparative Example 10;

[0032] Fig.13 This is a schematic diagram of the structure of the matrix block produced using the matrix block production process of Comparative Example 11. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] The present invention provides a technical solution: a process for producing a wood fiber cultivation matrix block, comprising the following steps:

[0036] S1. Chipping: The wood is processed into wood chips by a chipper;

[0037] S2. Screening: Screen the wood chips produced by the chipper and select the wood chips that meet the size requirements for the next process;

[0038] S3, hot grinding: the screened wood chips are subjected to high temperature cooking and mechanical separation to obtain fibers. The cooking temperature is 160°C and the average length of the fibers obtained by mechanical separation is 1 cm.

[0039] S4. Adding conditioners: Add conditioners according to planting needs;

[0040] S5, drying: drying the fiber by controlling the ambient temperature so that the moisture content of the fiber after drying is 10%;

[0041] S6. Paving: mechanical vacuum paving;

[0042] S7, pre-pressing: pre-pressing the soft slab;

[0043] S8, slab sawing: trimming and sawing the pre-pressed slab;

[0044] S9, hot pressing: heating and raising the temperature of the fiber mat, and applying pressure to densify the fluffy fiber mat, so as to press the fiber mat into shape; the hot pressing is divided into three stages: the first stage is to give high pressure to the mat to shape its upper and lower surfaces, the pressure is controlled at 1.8MPa, the time is 2-10s, preferably 10s; the second stage is to transfer heat from the surface temperature of the mat to the core, the pressure is controlled at 0.9MPa, the time is 60-80s, preferably 80s; the third stage is to solidify the mat as a whole and shape it with a fixed thickness, the pressure is controlled at 1.8MPa, the time is 60-80s, preferably 80s, and the temperature of the whole hot pressing process is controlled at 120°C;

[0045] S10, cooling: the hot-pressed fiberboard is cooled on a cooling panel turning machine;

[0046] S11. Sawing and processing according to different uses: sawing and cutting the fiberboard into the shapes of seedling blocks, cultivation blocks, planting blocks and substrate strips, and processing the planting holes on the upper parts.

[0047] Example 2

[0048] The present invention also provides a technical solution: a process for producing a wood fiber cultivation matrix block, comprising the following steps:

[0049] S1. Chipping: The wood is processed into wood chips by a chipper;

[0050] S2. Screening: Screen the wood chips produced by the chipper and select the wood chips that meet the size requirements for the next process;

[0051] S3, hot grinding: the screened wood chips are subjected to high temperature cooking and mechanical separation to obtain fibers. The cooking temperature is 170°C and the average length of the fibers obtained by mechanical separation is 2 cm.

[0052] S4. Adding conditioners: Add conditioners according to planting needs;

[0053] S5, drying: drying the fiber by controlling the ambient temperature so that the moisture content of the fiber after drying is 12%;

[0054] S6. Paving: mechanical vacuum paving;

[0055] S7, pre-pressing: pre-pressing the soft slab;

[0056] S8, slab sawing: trimming and sawing the pre-pressed slab;

[0057] S9, hot pressing: heating and raising the temperature of the fiber mat, and applying pressure to densify the fluffy fiber mat, so as to press the fiber mat into shape; the hot pressing is divided into three stages: the first stage is to give high pressure to the mat to shape its upper and lower surfaces, the pressure is controlled at 2MPa, the time is 2-10s, preferably 6s; the second stage is to transfer heat from the surface temperature of the mat to the core, the pressure is controlled at 1MPa, the time is 60-80s, preferably 70s; the third stage is to solidify the mat as a whole and shape it with a fixed thickness, the pressure is controlled at 2MPa, the time is 60-80s, preferably 70s, and the temperature of the whole hot pressing process is controlled at 130°C;

[0058] S10, cooling: the hot-pressed fiberboard is cooled on a cooling panel turning machine;

[0059] S11. Sawing and processing according to different uses: sawing and cutting the fiberboard into the shapes of seedling blocks, cultivation blocks, planting blocks and substrate strips, and processing the planting holes on the upper parts.

[0060] Example 3

[0061] The present invention also provides a technical solution: a process for producing a wood fiber cultivation matrix block, comprising the following steps:

[0062] S1. Chipping: The wood is processed into wood chips by a chipper;

[0063] S2. Screening: Screen the wood chips produced by the chipper and select the wood chips that meet the size requirements for the next process;

[0064] S3, hot grinding: the screened wood chips are subjected to high temperature cooking and mechanical separation to obtain fibers. The cooking temperature is 180°C and the average length of the fibers obtained by mechanical separation is 3 cm.

[0065] S4. Adding conditioners: Add conditioners according to planting needs;

[0066] S5, drying: drying the fiber by controlling the ambient temperature so that the moisture content of the fiber after drying is 15%;

[0067] S6. Paving: mechanical vacuum paving;

[0068] S7, pre-pressing: pre-pressing the soft slab;

[0069] S8, slab sawing: trimming and sawing the pre-pressed slab;

[0070] S9, hot pressing: heating and raising the temperature of the fiber mat, and applying pressure to densify the fluffy fiber mat, so as to press the fiber mat into shape; the hot pressing is divided into three stages: the first stage is to give high pressure to the mat to shape its upper and lower surfaces, and the pressure is controlled at 2.3MPa, the time is 2-10s, preferably 2s; the second stage is to transfer heat from the surface temperature of the mat to the core, and the pressure is controlled at 1.2MPa, the time is 60-80s, preferably 60s; the third stage is to solidify the mat as a whole and shape it with a fixed thickness, and the pressure is controlled at 2.1MPa, the time is 60-80s, preferably 60s, and the temperature of the whole hot pressing process is controlled at 140°C;

[0071] S10, cooling: the hot-pressed fiberboard is cooled on a cooling panel turning machine;

[0072] S11. Sawing and processing according to different uses: sawing and cutting the fiberboard into the shapes of seedling blocks, cultivation blocks, planting blocks and substrate strips, and processing the planting holes on the upper parts.

[0073] Comparative Example 1: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber board are as follows: the pressure applied to the board in the first stage is controlled at 1.7 MPa; the pressure applied to the board in the second stage is controlled at 0.4 MPa; the pressure applied to the board in the third stage is controlled at 1 MPa, and the temperature of the hot pressing process is controlled at 180°C throughout the process, and urea-formaldehyde glue is required to be added before hot pressing.

[0074] Comparative Example 2: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 3.4 MPa; the pressure applied to the blank in the second stage is controlled at 1.2 MPa; the pressure applied to the blank in the third stage is controlled at 2.1 MPa, and the temperature of the hot pressing process is controlled at 120°C throughout the process.

[0075] Comparative Example 3: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 1.5MPa; the pressure applied to the blank in the second stage is controlled at 1.2MPa; the pressure applied to the blank in the third stage is controlled at 2.1MPa, and the temperature of the hot pressing process is controlled at 120°C throughout the process.

[0076] Comparative Example 4: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 2.3 MPa; the pressure applied to the blank in the second stage is controlled at 1.9 MPa; the pressure applied to the blank in the third stage is controlled at 1.5 MPa, and the temperature of the hot pressing process is controlled at 140°C throughout the process.

[0077] Comparative Example 5: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 2.3 MPa; the pressure applied to the blank in the second stage is controlled at 0.6 MPa; the pressure applied to the blank in the third stage is controlled at 1.5 MPa, and the temperature of the hot pressing process is controlled at 140°C throughout the process.

[0078] Comparative Example 6: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 2.3MPa; the pressure applied to the blank in the second stage is controlled at 1MPa; the pressure applied to the blank in the third stage is controlled at 2.6MPa, and the temperature of the hot pressing process is controlled at 130°C throughout the process.

[0079] Comparative Example 7: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 2.3MPa; the pressure applied to the blank in the second stage is controlled at 1MPa; the pressure applied to the blank in the third stage is controlled at 1.5MPa, and the temperature of the hot pressing process is controlled at 130°C throughout the process.

[0080] Comparative Example 8: Compared with the matrix block production process of the present invention, the hot pressing stage of the fiber slab is as follows: the pressure applied to the slab is controlled at 2.6 MPa throughout the whole process; and the temperature of the hot pressing process is controlled at 140°C throughout the whole process.

[0081] Comparative Example 9: Compared with the matrix block production process of the present invention, the hot pressing stage of the fiber slab is as follows: the pressure applied to the slab is controlled at 0.8 MPa throughout the whole process; and the temperature of the hot pressing process is controlled at 140°C throughout the whole process.

[0082] Comparative Example 10: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 2MPa; the pressure applied to the blank in the second stage is controlled at 1MPa; the pressure applied to the blank in the third stage is controlled at 1.9MPa, and the temperature of the hot pressing process is controlled at 200°C throughout the process.

[0083] Comparative Example 11: Compared with the matrix block production process of the present invention, the hot pressing stages of the fiber blank are: the pressure applied to the blank in the first stage is controlled at 2.2 MPa; the pressure applied to the blank in the second stage is controlled at 1.1 MPa; the pressure applied to the blank in the third stage is controlled at 1.8 MPa, and the temperature of the hot pressing process is controlled at 100°C throughout the process.

[0084] Test verification: The production processes of Comparative Examples 1-11 and Examples 1-3 were respectively used to process the matrix blocks for comparative analysis. The test data are shown in Table 1:

[0085] Table 1 Comparative experimental data of matrix blocks produced by different hot pressing processes

[0086]

[0087]

[0088]

[0089] From Table 1 we can see that:

[0090] The matrix blocks produced by the matrix block production processes of Examples 1, 2 and 3 are as follows: Figure 1 and Figure 2 As shown, there is no need to add glue, there is no pre-curing layer, the cross-sectional density distribution of the matrix block is balanced in the compressed state, the time required to absorb water to the saturated state is short, the thickness expansion multiples after absorbing water to the saturated state are large, and the matrix block after expansion has a soft texture, many pores, good water retention performance, easy degradation, and is suitable for soilless cultivation of plants.

[0091] The matrix block produced by the matrix block production process of Comparative Example 1 is as follows Figure 3As shown, urea-formaldehyde glue needs to be added. The internal fibers are tightly combined. The density of the upper and lower layers of the matrix block in the compressed state is greater than the density of the middle layer. The cross-sectional density distribution is uneven. It takes a long time to absorb water to the saturated state. The thickness expansion is small when absorbing water to the saturated state. There are few pores and it contains formaldehyde. It is not suitable for plant growth, so it cannot be used as a matrix.

[0092] The matrix block produced by the matrix block production process of Comparative Example 2 is as follows: Figure 4 As shown, due to the excessively high pressure in the first stage, the upper and lower surfaces solidify rapidly to form a high-density hardened layer, and the upper and lower surfaces are too hard to be used as a matrix block.

[0093] The matrix block produced by the matrix block production process of Comparative Example 3 is as follows: Figure 5 As shown, due to the low pressure in the first stage, the upper and lower surfaces of the matrix plate became soft and fell off, making it unsuitable for use as a matrix block.

[0094] The matrix block produced by the matrix block production process of Comparative Example 4 is as follows Figure 6 As shown, due to the excessive pressure in the second stage, the gaps between the fibers become smaller, making heat transfer difficult, resulting in the matrix board being layered up and down at the core, and the bonding force in the middle is extremely poor, and can be easily torn into two by hand, making it unsuitable for use as a matrix block.

[0095] The matrix block produced by the matrix block production process of Comparative Example 5 is as follows: Figure 7 As shown, the upper and lower surfaces of the matrix plate are normally solidified in the first stage, but the pressure in the second stage is too small, resulting in serious multi-layering of the matrix plate and cracking of the three-layer structure, which is not suitable for use as a matrix block.

[0096] The matrix block produced by the matrix block production process of Comparative Example 6 is as follows: Figure 8 As shown, due to the excessively high pressure in the third stage, the pressed substrate board core is very dense and cannot be soaked with water, making it unsuitable for plant rooting, that is, it is not suitable for use as a substrate block.

[0097] The matrix block produced by the matrix block production process of Comparative Example 7 is as follows: Fig. 9 As shown, since the pressure in the third stage is too low, it is not enough to press the matrix slab into a plate-like structure, and it is very soft and cannot be used as a matrix block foundation.

[0098] The matrix block produced by the matrix block production process of Comparative Example 8 is as follows: Fig.10 As shown, since the pressure in each stage is too high, the pressed matrix plate is separated into upper and lower layers, and the upper and lower layers are too thick hard shells, which are not suitable for use as matrix blocks.

[0099] The matrix block produced by the matrix block production process of Comparative Example 9 is as follows: Fig.11As shown, due to insufficient pressure at each stage, the binding force between the fibers themselves is not enough to press them into a plate shape and cannot be used as a base for a matrix block.

[0100] The matrix block produced by the matrix block production process of Comparative Example 10 is as follows Fig.12 As shown, due to the high temperature during the entire hot pressing process, a large amount of moisture in the matrix board vaporizes and accumulates in the core of the board, which not only causes severe carbonization of the upper and lower surfaces, but also causes delamination and cracking of the upper and lower layers, making it impossible to use as the foundation of the matrix block.

[0101] The matrix block produced by the matrix block production process of Comparative Example 11 is as follows Fig.13 As shown, since the temperature during the entire hot pressing process is too low, the matrix plate cannot be pressed into shape and is overall soft and cannot be used as a matrix block foundation.

[0102] The substrate block processed by the production process of the wood fiber cultivation substrate block of the present invention is low in cost and good in degradability because it is processed by wood fiber, and will not cause secondary pollution to the environment; the time required for absorbing water to a saturated state is short, the substrate is relatively soft when absorbing water to a saturated state, the number of gaps when absorbing water to a saturated state is large, the water absorption and fertilizer retention performance is good, and the substrate is suitable for plant seedling and cultivation; the expansion multiple of the substrate block when absorbing water to a saturated state is high, and the substrate block is in a compressed state before use, which is convenient for transportation.

[0103] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for producing wood fiber cultivation substrate blocks, characterized in that: The following steps are involved: S1, chipping: chipping wood into wood chips; S2. Screening: Screen the wood chips and select the wood chips that meet the size requirements for the next process; S3, hot grinding: the screened wood chips are steamed at high temperature and mechanically separated to obtain fibers; S4, drying: drying the fibers by passing hot air; S5. Paving: mechanical vacuum paving; S6, pre-pressing: pre-pressing the soft slab; S7, slab sawing: trimming and sawing the pre-pressed slab; S8, hot pressing: heating the fiber mat and applying pressure to densify the fluffy fiber mat, so as to press the fiber mat into shape; the hot pressing is divided into three stages: the first stage applies high pressure to the mat to shape its upper and lower surfaces, and the pressure is controlled between 1.8 and 2.3 MPa; the second stage makes the surface temperature of the mat transfer heat to the core, and the pressure is controlled between 0.9 and 1.2 MPa; the third stage is to solidify the mat as a whole and shape it into a fixed thickness, and the pressure is controlled between 1.8 and 2.1 MPa, and the temperature of the whole hot pressing process is controlled between 120℃ and 140℃; S9, cooling: cooling the hot-pressed fiberboard; S10. Sawing and processing according to different uses: sawing and cutting the fiberboard into the shapes of seedling blocks, cultivation blocks, planting blocks and substrate strips, and processing the planting holes on the upper parts thereof.

2. A process for producing wood fiber cultivation matrix blocks according to claim 1, characterized in that: The cooking temperature in step S2 is 160°C to 180°C.

3. The process for producing a wood fiber cultivation matrix block according to claim 1, characterized in that: The average length of the fibers obtained by mechanical separation in step S2 is 1 to 3 cm.

4. The process for producing a wood fiber cultivation matrix block according to claim 1, characterized in that: After the hot grinding in step S3, a conditioner may be added according to planting needs.

5. The process for producing a wood fiber cultivation matrix block according to claim 1, characterized in that: The moisture content of the fiber after drying in step S4 is between 10% and 15%.

6. The process for producing a wood fiber cultivation matrix block according to claim 1, characterized in that: The fiberboard formed by hot pressing in step S9 is cooled on a cooling panel turning machine.

Citation Information

Patent Citations

  • Composite type alien earth sparging wood fiber, and fabricating method

    CN1958718A

  • Full environmental-protection and full degradation plant fiber flower container and production process thereof

    CN101563991A

  • Hot-pressing technology for manufacturing board by utilizing crop straws

    CN101670608A

  • Biological matrix pressing block

    CN104170704A

  • Method for preparing plate-type straw biological seedling culture medium with dry process

    CN106465655A