Hemostatic aerogel and preparation method thereof

By forming a spiral channel structure in the hemostatic aerogel, the problem of reduced mechanical strength of existing hemostatic aerogels after absorbing blood is solved, a more efficient and stable hemostatic effect is achieved, and the modern medical requirements for high efficiency, safety and ease of use are achieved. needs.

CN118767200APending Publication Date: 2024-10-15DONGHUA UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410805863.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The mechanical strength of existing hemostatic aerogels decreases after absorbing blood, resulting in unstable hemostatic effects, harmful reactions to tissues and usage restrictions, making it difficult to meet the needs of modern medical care for efficiency, safety, and ease of use.

Method used

A fiber suspension of dispersed hydrophilic fiber materials and hydrophobic fiber materials is prepared by shearing. After freeze-drying, cross-linking is initiated to form a hemostatic aerogel with a spiral channel structure. The channel structure is controlled to improve porosity and pore connectivity. , enhance water absorption and blood coagulation efficiency.

Benefits of technology

Significantly improves the hemostatic performance of hemostatic aerogels, increases porosity and pore connectivity, promotes rapid blood absorption and coagulation, provides better mechanical support, extends the long-term stability of hemostatic materials, and reduces blood loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767200A_ABST
    Figure CN118767200A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hemostatic materials, and relates to hemostatic aerogel and a preparation method thereof. The preparation method comprises the following steps: shearing by a shearing machine to prepare a fiber suspension in which a hydrophilic fiber material and a hydrophobic fiber material are dispersed and in which a cross-linking agent is dissolved, freezing the fiber suspension until the fiber suspension is completely frozen, freeze-drying, initiating cross-linking, or further performing post-treatment to obtain the hemostatic aerogel. The water contact angle of the hydrophilic fiber material is 30-80 degrees, the shear stiffness is 10-20, and the length-diameter ratio is greater than or equal to 40; the water contact angle of the hydrophobic fiber material is 100-140 degrees, the shear stiffness is 0.1-0.5, and the length-diameter ratio is greater than or equal to 40; the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is (1-2): 1; the shearing speed of the shearing machine is 10000 to 15000 rpm (revolutions per minute); the supercooling degree during freezing is greater than or equal to 5.5 DEG C; the prepared hemostatic aerogel has a spiral pore channel. The preparation method of the hemostatic aerogel is simple, and the prepared hemostatic aerogel is good in hemostatic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hemostatic materials and relates to a hemostatic aerogel and a preparation method thereof. Background Art

[0002] In the field of medical emergency, the development of hemostatic materials has always received widespread attention. With the intensification of the aging trend of the population and the continuous advancement of surgical techniques, the demand for hemostatic materials is increasing, especially when dealing with large-scale, irregular, deep cavities and complex wounds involving important functional tissues. Traditional hemostatic technology can no longer meet the needs of modern medicine. Massive blood loss in battlefields and daily acute trauma is one of the main causes of shock, organ failure and high mortality. Therefore, the development of efficient, safe and easy-to-use hemostatic materials is of great practical significance.

[0003] At present, widely used hemostatic materials include mechanical, mechanical pressure, chemical and biological factor materials, but these materials all have certain application limitations. Mechanical hemostatic materials such as hemostatic forceps cannot be effectively applied inside the wound, and it is difficult to control bleeding from deep wounds; mechanical pressure hemostatic products may cause organ compression complications; chemical hemostatic materials may produce reaction heat that is harmful to tissues or have limited efficacy; biological factor hemostatic materials have usage restrictions, such as they should not be used by patients with coagulation dysfunction, and may cause foreign body or allergic reactions. In addition, some hemostatic materials are expensive, difficult to store, difficult to remove from the wound, or cause secondary damage to the wound, which limits their clinical application.

[0004] As an emerging hemostatic material, aerogel hemostatic material can quickly absorb a large amount of blood in a humid environment due to its high porosity and large specific surface area, and promote blood coagulation through physical compression and chemical action, thereby improving hemostatic efficiency. However, the hemostatic performance of aerogel hemostatic materials currently on the market needs to be further improved.

[0005] For example, patent application CN115212344B discloses a self-expanding hemostatic aerogel and a preparation method thereof. The patent utilizes gas expansion to produce a pulsed jet effect to deliver drugs to hidden bleeding points and micro-groove bleeding points deep in the wound, and utilizes the convection effect caused by gas jets to promote drug diffusion inside the wound, increase the contact area between the drug and coagulation substances, and accelerate thrombosis. However, the self-expanding hemostatic aerogel prepared by the patent loses some of its mechanical strength after absorbing blood, resulting in unstable hemostatic effect.

[0006] In summary, although aerogel hemostatic materials show good application prospects in the field of hemostasis, their hemostatic performance still needs to be improved. Summary of the invention

[0007] The purpose of the present invention is to solve the problems existing in the prior art and provide a hemostatic aerogel and a preparation method thereof.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a hemostatic aerogel comprises preparing a fiber suspension in which a hydrophilic fiber material and a hydrophobic fiber material are dispersed and a crosslinking agent is dissolved by shearing with a shearing machine, freezing the fiber suspension until it is completely frozen, freeze-drying it, inducing crosslinking, or further performing post-treatment to obtain a hemostatic aerogel;

[0010] The water contact angle of the hydrophilic fiber material is 30° to 80°, the shear stiffness is 10 to 20, and the aspect ratio is ≥40; the water contact angle of the hydrophobic fiber material is 100° to 140°, the shear stiffness is 0.1 to 0.5, and the aspect ratio is ≥40; the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is 1 to 2:1; the shear rate of the shearing machine is 10000 to 15000 rpm; the supercooling degree during freezing is ≥5.5°C.

[0011] In the preparation process of the present invention, the pore structure in the hemostatic aerogel is regulated by regulating the characteristic parameters (water contact angle, shear stiffness and aspect ratio) of the hydrophilic fiber material, the characteristic parameters (water contact angle, shear stiffness and aspect ratio) of the hydrophobic fiber material, the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material, the shear rate of the shearing machine, and the supercooling degree during freezing, so that the pores are spiral pores.

[0012] As the preferred technical solution:

[0013] In the preparation method of the hemostatic aerogel as described above, the preparation process of the fiber suspension is: the hydrophilic fiber material and the hydrophobic fiber material are dispersed in water, and after shearing with a shearing machine for 5 to 8 minutes, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 3 to 5 minutes to obtain a fiber suspension.

[0014] In the method for preparing a hemostatic aerogel as described above, the hydrophilic fiber material is cellulose fiber or cellulose derivative fiber; the hydrophobic fiber material is thermoplastic polyurethane fiber, polylactic acid fiber or polycaprolactone fiber; and the crosslinking agent in the crosslinking agent aqueous solution is a crosslinking agent containing epoxy groups, amino groups or carboxyl groups.

[0015] In the method for preparing a hemostatic aerogel as described above, the content of the hydrophilic fiber material in the fiber suspension is 0.5-0.67 wt %.

[0016] In the method for preparing a hemostatic aerogel as described above, the content of the crosslinking agent in the fiber suspension is 0.25-0.5 wt %.

[0017] In the method for preparing a hemostatic aerogel as described above, freezing the fiber suspension until it is completely frozen means leaving the fiber suspension at -50 to -196°C for 0.2 to 8 hours.

[0018] In the method for preparing the hemostatic aerogel as described above, cross-linking is initiated by heating, the heating temperature is 40 to 120° C., and the heating time is 2 to 4 hours.

[0019] The present invention also provides a hemostatic aerogel prepared by the method for preparing a hemostatic aerogel as described in any one of the above items, and the aerogel has a spiral pore.

[0020] As the preferred technical solution:

[0021] The hemostatic aerogel as described above has a porosity of 64-92% and a pore size (not only the spiral pores, but also other pores in the hemostatic aerogel) of 2-30 μm.

[0022] The hemostatic aerogel as described above has a BCI value of 0.6-3%, a water absorption rate of 1328-4197%, a blood absorption rate of 885-1708%, an average hemostasis time of 30-120s and an average blood loss of 250-882mg in a rat tail amputation wound model.

[0023] Principle of the invention:

[0024] The hemostatic performance of the hemostatic aerogel of the present invention is significantly better than that of the hemostatic aerogel in the prior art, because the present invention adopts a spiral pore aerogel with a periodic hydrophilic-hydrophobic gradient distribution, and the spiral pore structure helps to improve the porosity and pore connectivity of the aerogel, which is crucial for the rapid absorption and coagulation of blood.

[0025] The spiral pore structure can enhance capillary action and promote the flow and diffusion of water in the pores. The spiral pores combined with the hydrophilic-hydrophobic gradient can guide the directional flow and distribution of the liquid, reduce the energy consumption in the transmission process, promote the transmission of water, and accelerate the diffusion rate of water in the blood into the aerogel, thereby improving the water absorption capacity, helping to concentrate the blood and activate coagulation factors; the spiral pore structure can also increase the contact area between the aerogel and the liquid, enhance the interaction between the aerogel and the blood, extend the blood transmission path, improve the coagulation efficiency, and promote the formation of blood clots, thereby reducing blood loss; in addition, due to its unique geometric shape, the spiral pore structure can more effectively fit the irregular wound surface when pressure is applied, provide uniform compression force, and help to quickly stop bleeding; and provide better mechanical support for the material, improving the long-term stability of the hemostatic material after absorbing blood.

[0026] When preparing aerogels with spiral pore structures, the dispersion medium (fiber) in deionized water has different effects on water because of the different hydrophilicity and hydrophobicity of the fiber itself. Hydrophilic fibers usually contain polar groups on their surface, which are easy to form hydrogen bonds with water and have strong interactions with water molecules. They expand in water to increase the contact area with water, are not easy to aggregate in the fluid, and have better dispersibility because their movement in the fluid is less hindered by water molecules. Hydrophilic fibers are more likely to be oriented under the high-speed shearing action of the fluid and dispersed in deionized water. Hydrophobic fibers tend to avoid contact with water and are more likely to float in water. Under high-speed shear, hydrophobic fiber materials (low shear stiffness) tend to aggregate and sink, and their sedimentation speed is faster than that of hydrophilic fiber materials (high shear stiffness). In addition, because hydrophobic fiber materials with low shear stiffness are more susceptible to the influence of redirection torque in shear flow than hydrophilic fiber materials with high shear stiffness, the arrangement direction of hydrophobic fiber materials deviates from the direction of gravity (i.e., the Z-axis direction), while the arrangement direction of hydrophilic fiber materials is close to being parallel to the direction of gravity (i.e., the Z-axis direction). All fiber materials are distributed in a petal-like shape with the axial direction. The more hydrophilic the hydrophilic fiber material is, the more it is in the upper layer, and the angle with the Z axis is closer to 30°~60°. The more hydrophobic the hydrophobic fiber material is, the closer it is to the horizontal axis, and the angle with the Z axis is closer to 60°~90°, forming a hydrophilic-hydrophobic gradient (such as Fig.10 As shown). Under high supercooling, the growth rate of ice crystals in the vertical direction is greater than the growth rate in the horizontal direction, and the ice crystals grow vertically to the surface of the fiber material (as shown in Fig.11 As shown). During the freezing process, the binding energy of water molecules on the hydrophilic fiber is lower, and the rapid migration of water molecules and the formation of hydrogen bonds make it freeze faster. The water droplets on the hydrophobic fiber tend to remain spherical, and the contact area with water is relatively small, so it remains unfrozen for a long time, thereby delaying the growth of ice crystals. The hydrophobic fiber exhibits a slower freezing rate because the migration of water molecules is hindered and the formation of hydrogen bonds is slow. This difference causes the ice crystals to grow preferentially along the direction of the hydrophilic fiber, thus forming an orientation (as shown). Fig.12 As shown in a, the hydrophilic fibers are distributed close to the longitudinal Z axis, while the hydrophobic fibers are distributed away from the longitudinal Z axis, that is, they are mostly distributed in the horizontal direction. The hydrophilic and hydrophobic gradient formed by the hydrophilic and hydrophobic fiber materials pulls the ice sheet layer to extend continuously in the hydrophobic direction (as shown in a). Fig.12 Middle b, Fig.12 After freeze drying, ice crystals sublimate to obtain stepped spiral channels.

[0027] Beneficial effects:

[0028] In the preparation process of the present invention, the pore structure in the hemostatic aerogel is regulated by regulating the characteristic parameters of the hydrophilic fiber material (water contact angle, shear stiffness and aspect ratio), the characteristic parameters of the hydrophobic fiber material (water contact angle, shear stiffness and aspect ratio), the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material, the shear rate of the shearing machine and the supercooling degree during freezing, so that the pores are spiral pores, thereby giving the hemostatic aerogel excellent hemostatic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a micro-CT scanning diagram of the spiral pore distribution of the hemostatic aerogel prepared in Example 1;

[0030] Figure 2 This is a physical picture of the hemostatic aerogel prepared in Example 1 (the arrows in the figure indicate the distribution of spiral channels);

[0031] Figure 3 It is a comparison chart of the BCI values ​​of the hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in each embodiment under the same test conditions;

[0032] Figure 4 It is a comparison chart of water absorption of hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in each embodiment under the same test conditions;

[0033] Figure 5 This is a comparison chart of the blood absorption rates of the hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in each embodiment under the same test conditions;

[0034] Figure 6 It is a comparison chart of the average hemostatic time of the hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in each embodiment under the same test conditions in a rat tail amputation wound model;

[0035] Figure 7 This is a comparison chart of the average blood loss of the hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in each embodiment under the same test conditions in a rat tail amputation wound model;

[0036] Figure 8 This is a comparison chart of the average hemostatic time of the hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in Example 1 in a mouse liver penetrating wound model under the same test conditions;

[0037] Fig. 9 This is a comparison chart of the average blood loss of the hemostatic aerogel, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze prepared in Example 1 under the same test conditions in a mouse liver penetrating wound model;

[0038] Fig.10This is the front view of fiber distribution;

[0039] Fig.11 It is a front view to illustrate the growth of ice crystals;

[0040] Fig.12 Schematic diagram of ice crystal growth; wherein, a is a front view of ice crystals preferentially growing along hydrophilic fibers, b is a front view of ice crystals extending and growing along the hydrophilic-hydrophobic gradient toward the hydrophobic direction, and c is a front view of ice crystals extending and growing along the hydrophilic-hydrophobic gradient toward the hydrophobic direction. DETAILED DESCRIPTION

[0041] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0042] The following are the test methods for the relevant performance indicators in each embodiment:

[0043] Porosity (P): Density ρ (g / cm 3 ), volume V(cm 3 ) was cut and weighed, recorded as W0 (g); then it was immersed in 30 mL of anhydrous ethanol solution, and the air in the pores of the hemostatic aerogel was removed by vacuum. After 30 minutes, it was carefully taken out and the residual ethanol on the surface was wiped with filter paper to keep the hemostatic aerogel from dripping liquid. Its mass was weighed and recorded as W1 (g). The porosity P was calculated as follows:

[0044] P(%)=(W1-W0) / (ρV)×100%.

[0045] BCI value: 200 μL and 20 μL of CaCl2 solution (solute is CaCl2, solvent is deionized water, concentration is 0.2 mol / L) were added to 50 mg of hemostatic aerogel preheated for 15 min in sequence, incubated at 37 °C for 10 min, and 25 mL of deionized water was slowly added to lyse the blood cells not bound to the hemostatic aerogel without destroying the thrombus. After 5 min, the absorbance OD of the supernatant was measured at a wavelength of 540 nm on the microplate reader. A mixture of 200 μL of sodium citrate anticoagulated whole blood and 25 mL of deionized water was used as a blank control. Each group was tested 6 times. The BCI value calculation formula is as follows:

[0046] BCI (%) = [OD] 样 / [OD] 空 ×100%;

[0047] Where, [OD] 样is the average absorbance of the experimental group, [OD] 空 is the average absorbance of the blank control group.

[0048] Water absorption (P w ): Cut the hemostatic aerogel and weigh it, record it as w0 (mg), then soak it in 30mL of deionized water, take it out carefully after soaking for 30min, wipe the residual water on the surface with filter paper, keep the hemostatic aerogel without dripping liquid, weigh its mass, record it as w1 (mg), the sample water absorption rate P w The calculation formula is as follows:

[0049]

[0050] Blood sucking rate (P b ): Cut the hemostatic aerogel sample and weigh it, record it as W0 (mg); then soak it in 30mL sodium citrate anticoagulated whole blood, soak it for 30min and carefully take it out, hang it in the air until no blood drips on the surface, weigh its mass, record it as W1 (mg), and the sample blood absorption rate P b The calculation is as follows:

[0051] P b (%) = (W1-W0) / W0×100%.

[0052] Average hemostasis time and average blood loss in the mouse liver penetrating wound model: C57BL / 6J male mice were first randomly divided into five groups (3 mice in each group): control group, hemostatic cotton ball (manufacturer: Zhende Medical Supplies Co., Ltd.) group, hemostatic gelatin sponge (manufacturer: Jiangxi Xiangen Medical Technology Development Co., Ltd.) group, hemostatic gauze (manufacturer: Zhende Medical Supplies Co., Ltd.) group and sample (i.e., hemostatic aerogel) group. After the mice were anesthetized by nasal inhalation of isoflurane, they were fixed on a surgical soft board, and then the mouse liver was exposed through an abdominal incision, and the serous fluid around the liver was carefully removed to prevent affecting the blood loss test, and then a weighed filter paper (weight was recorded as W) was placed under the mouse liver in advance. f , unit mg), then use a 3mm diameter puncher to penetrate the mouse liver, and start timing immediately, and at the same time, apply the pre-weighed hemostatic material (i.e., hemostatic cotton ball, hemostatic gelatin sponge, hemostatic gauze or hemostatic aerogel, weight recorded as W0, unit mg) to the hemostatic site (i.e., the perforated site of the mouse liver) to stop bleeding (the control group does not stop bleeding), observe the bleeding of the liver every 15 seconds until the wound stops bleeding and the hemostasis is completed, then stop timing (i.e., the hemostasis time, unit s), weigh the filter paper and hemostatic material after blood absorption (the whole weight is recorded as W1, unit mg); during the experiment, record the amount of blood loss during the hemostasis process of three mice in each group (recorded as W, by the formula W=W1-W f-W0 was calculated, unit mg) and hemostasis time, and the average value was taken to obtain the average hemostasis time (s) and average blood loss (mg) of each group.

[0053] Average hemostasis time and average blood loss in the rat tail amputation wound model: SD rats (weighing 250-300 g) were first randomly divided into five groups (3 rats in each group): control group, hemostatic cotton ball (manufacturer: Zhende Medical Supplies Co., Ltd.) group, hemostatic gelatin sponge (manufacturer: Jiangxi Xiangen Medical Technology Development Co., Ltd.) group, hemostatic gauze (manufacturer: Zhende Medical Supplies Co., Ltd.) group, and sample (i.e., hemostatic aerogel) group. After the mice were anesthetized by nasal inhalation of isoflurane, the rats were fixed on a surgical soft board, and then the tail was cut off 3 cm from the tip of the rat's tail with surgical scissors to allow the rat's tail to bleed freely for 15 seconds. At the same time, filter paper 1 (filter paper 1 was stored in a ziplock bag 1, and the filter paper 1 was weighed in advance, and the weight was recorded as w1, in mg) was used to absorb the blood. After free bleeding for 15 seconds, the filter paper 1 after absorbing blood was weighed (the weight was recorded as W1, in mg), and the blood loss before treatment was calculated (recorded as W, in mg, W=W1-w1, if W If the blood loss is greater than 150 mg or less than 50 mg, it is considered abnormal, the data is discarded, and the experiment is repeated with a new SD rat). At the same time, the rat tail is quickly placed in a centrifuge tube (the centrifuge tube containing the hemostatic material is weighed in advance, and the weight is recorded as W2, in mg) filled with hemostatic materials (i.e., hemostatic cotton balls, hemostatic gelatin sponges, hemostatic gauze or hemostatic aerogel) for hemostasis (the control group is not subjected to hemostasis), and the timing is started. During the hemostasis process, filter paper 2 (centrifuge tube containing hemostatic materials) is used in time. The rat tail was stored together with filter paper 2 in a ziplock bag 2, the weight of filter paper 2 was recorded as w2, in mg), the spilled blood was wiped off, and the bleeding of the rat tail was observed every 15 s until the bleeding stopped (after the hemostasis was completed, the total weight of the ziplock bag 2 containing the hemostatic material and filter paper 2 was W2', in mg), the timing was ended (that is, the hemostasis time was obtained, in s), the blood loss during the hemostasis process was calculated (recorded as W', in mg, W'=W2'-W2-w2), and the total blood loss (W 总 =W+W'); during the experiment, the total blood loss and hemostasis time of the three rats in each group during the hemostasis process were recorded, and the average value was taken to obtain the average hemostasis time (s) and average blood loss (mg) of each group.

[0054] Example 1

[0055] A method for preparing a hemostatic aerogel, the specific steps are as follows:

[0056] (1) Preparation of raw materials;

[0057] Hydrophilic fiber material: cellulose acetate fiber, water contact angle of 30° to 75°, shear stiffness of 10 to 20, aspect ratio of 40 to 60;

[0058] Hydrophobic fiber material: thermoplastic polyurethane fiber, water contact angle of 100° to 140°, shear stiffness of 0.1 to 0.3, aspect ratio of 40 to 80;

[0059] water;

[0060] Cross-linking agent aqueous solution: The cross-linking agent is a blocked aqueous isocyanate (manufacturer is China Changzhou Houding Chemical Co., Ltd., model number is HD-8035);

[0061] (2) a hydrophilic fiber material and a hydrophobic fiber material in a mass ratio of 2:1 are dispersed in water, and after shearing for 5 minutes by a shearing machine, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 5 minutes to obtain a fiber suspension; wherein the shearing rate of the shearing machine is 13000 rpm; the content of the hydrophilic fiber material in the fiber suspension is 0.67 wt%, and the content of the crosslinking agent is 0.25 wt%;

[0062] (3) The fiber suspension was allowed to stand at -50°C (supercooling degree was 5.5°C) for 8 h, freeze-dried (temperature was -45°C, pressure was 15 Pa, time was 24 h), and then heated to induce cross-linking to obtain the hemostatic aerogel 1-1; wherein the heating temperature was 120°C and the time was 2 h.

[0063] The final hemostatic aerogel 1-1 is as follows Figure 2 As shown, the hemostatic aerogel 1-1 has a spiral channel (the micro-CT scanning result of the spiral channel is shown in Figure 1 The porosity of the hemostatic aerogel is 92%, and the pore size is 2-20 μm; the BCI value of the hemostatic aerogel 1-1 is 0.6%, the water absorption rate is 4197%, and the blood absorption rate is 885%; the average hemostasis time of the hemostatic aerogel 1-1 in the mouse liver penetrating wound model is 30 s and the average blood loss is 35 mg, and the average hemostasis time in the rat tail amputation wound model is 30 s and the average blood loss is 250 mg.

[0064] Under the same test conditions, the comparison of the average hemostatic time and average blood loss of hemostatic aerogel 1-1, hemostatic cotton balls, hemostatic gelatin sponges and hemostatic gauze in the mouse liver penetrating wound model is shown in Figure 2. Figure 8 , Fig. 9 shown.

[0065] Example 2

[0066] (1) Preparation of raw materials;

[0067] Hydrophilic fiber material: cellulose acetate fiber, water contact angle of 30° to 75°, shear stiffness of 10 to 20, aspect ratio of 40 to 60;

[0068] Hydrophobic fiber material: thermoplastic polyurethane fiber, water contact angle of 100° to 140°, shear stiffness of 0.1 to 0.3, aspect ratio of 40 to 80;

[0069] water;

[0070] Cross-linking agent aqueous solution: The cross-linking agent is a blocked aqueous isocyanate (manufacturer is China Changzhou Houding Chemical Co., Ltd., model number is HD-8035);

[0071] (2) a hydrophilic fiber material and a hydrophobic fiber material in a mass ratio of 1:1 are dispersed in water, and after shearing for 5 minutes by a shearing machine, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 5 minutes to obtain a fiber suspension; wherein the shearing rate of the shearing machine is 13000 rpm; the content of the hydrophilic fiber material in the fiber suspension is 0.5 wt %, and the content of the crosslinking agent is 0.25 wt %;

[0072] (3) The fiber suspension was allowed to stand at -50°C (supercooling degree was 5.5°C) for 8 h, freeze-dried (temperature was -45°C, pressure was 15 Pa, time was 24 h), and then heated to induce cross-linking to obtain hemostatic aerogel 1-2; wherein the heating temperature was 120°C and the time was 2 h.

[0073] The final hemostatic aerogel 1-2 has spiral pores; the porosity of the hemostatic aerogel 1-2 is 85%, and the pore size is 3.5-10 μm; the BCI value of the hemostatic aerogel 1-2 is 0.8%, the water absorption rate is 3350%, and the blood absorption rate is 1139%; the average hemostasis time of the hemostatic aerogel 1-2 in the rat tail amputation wound model is 75 s and the average blood loss is 263 mg.

[0074] Example 3

[0075] (1) Preparation of raw materials;

[0076] Hydrophilic fiber material: cellulose acetate fiber, water contact angle of 30° to 75°, shear stiffness of 10 to 20, aspect ratio of 40 to 60;

[0077] Hydrophobic fiber material: thermoplastic polyurethane fiber, water contact angle of 100° to 140°, shear stiffness of 0.1 to 0.3, aspect ratio of 40 to 80;

[0078] water;

[0079] Cross-linking agent aqueous solution: The cross-linking agent is a blocked aqueous isocyanate (manufacturer is China Changzhou Houding Chemical Co., Ltd., model number is HD-8035);

[0080] (2) a hydrophilic fiber material and a hydrophobic fiber material in a mass ratio of 2:1 are dispersed in water, and after shearing for 5 minutes by a shearing machine, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 5 minutes to obtain a fiber suspension; wherein the shearing rate of the shearing machine is 13000 rpm; the content of the hydrophilic fiber material in the fiber suspension is 0.67 wt%, and the content of the crosslinking agent is 0.5 wt%;

[0081] (3) The fiber suspension was allowed to stand at -50°C (supercooling degree was 5.5°C) for 8 h, freeze-dried (temperature was -45°C, pressure was 15 Pa, time was 24 h), and then heated to induce cross-linking to obtain hemostatic aerogel 1-3; wherein the heating temperature was 120°C and the time was 2 h.

[0082] The final hemostatic aerogel 1-3 has spiral pores; the porosity of the hemostatic aerogel 1-3 is 64%, and the pore size is 2 to 20 μm; the BCI value of the hemostatic aerogel 1-3 is 2.6%, the water absorption rate is 1328%, and the blood absorption rate is 1220%; the average hemostatic time of the hemostatic aerogel 1-3 in the rat tail amputation wound model is 120 s and the average blood loss is 882 mg.

[0083] Example 4

[0084] A method for preparing a hemostatic aerogel, the specific steps are as follows:

[0085] (1) Preparation of raw materials;

[0086] Hydrophilic fiber material: cellulose fiber, water contact angle of 30° to 80°, shear stiffness of 10 to 20, aspect ratio of 40 to 60;

[0087] Hydrophobic fiber material: polylactic acid fiber, water contact angle of 100° to 128°, shear stiffness of 0.1 to 0.5, aspect ratio of 40 to 80;

[0088] water;

[0089] Deionized water;

[0090] Cross-linking agent aqueous solution: the cross-linking agent is sodium citrate (CAS No. 68-04-2);

[0091] (2) A hydrophilic fiber material and a hydrophobic fiber material in a mass ratio of 2:1 are dispersed in water, and after shearing for 6 minutes by a shearing machine, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 4 minutes to obtain a fiber suspension; wherein the shearing rate of the shearing machine is 10000 rpm; the content of the hydrophilic fiber material in the fiber suspension is 0.67wt%, and the content of the crosslinking agent is 0.5wt%;

[0092] (3) The fiber suspension was allowed to stand at -70°C (supercooling degree was 7°C) for 6 h, freeze-dried (temperature was -50°C, pressure was 20 Pa, time was 36 h), and then heated to induce crosslinking. After the crosslinking was completed, the fiber suspension was cooled to room temperature to obtain a crosslinked product, which was packaged in a dialysis bag and immersed in deionized water. The deionized water was replaced every 8 h until the pH value of the immersion liquid was neutral, thereby obtaining hemostatic aerogel 2-1; wherein, the heating temperature was 80°C and the time was 3 h.

[0093] The finally prepared hemostatic aerogel 2-1 has spiral pores; the porosity of the hemostatic aerogel 2-1 is 73%, and the pore size is 2-10 μm; the BCI value of the hemostatic aerogel 2-1 is 3%, the water absorption rate is 1915%, and the blood absorption rate is 1042%; the average hemostatic time of the hemostatic aerogel 2-1 in the mouse liver penetrating wound model is 60 s and the average blood loss is 48 mg, and the average hemostatic time in the rat tail amputation wound model is 90 s and the average blood loss is 636 mg.

[0094] Example 5

[0095] A method for preparing a hemostatic aerogel, the specific steps are as follows:

[0096] (1) Preparation of raw materials;

[0097] Hydrophilic fiber material: cellulose fiber, water contact angle of 30° to 80°, shear stiffness of 10 to 20, aspect ratio of 40 to 60;

[0098] Hydrophobic fiber material: polylactic acid fiber, water contact angle of 100° to 128°, shear stiffness of 0.1 to 0.5, aspect ratio of 40 to 80;

[0099] water;

[0100] Deionized water;

[0101] Cross-linking agent aqueous solution: the cross-linking agent is sodium citrate (CAS No. 68-04-2);

[0102] (2) a hydrophilic fiber material and a hydrophobic fiber material in a mass ratio of 1:1 are dispersed in water, and after shearing for 6 minutes by a shearing machine, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 4 minutes to obtain a fiber suspension; wherein the shearing rate of the shearing machine is 10000 rpm; the content of the hydrophilic fiber material in the fiber suspension is 0.5 wt%, and the content of the crosslinking agent is 0.5 wt%;

[0103] (3) The fiber suspension was allowed to stand at -70°C (supercooling degree was 7°C) for 6 h, freeze-dried (temperature was -50°C, pressure was 20 Pa, time was 36 h), and then heated to induce crosslinking. After the crosslinking was completed, the fiber suspension was cooled to room temperature to obtain a crosslinked product, which was packaged in a dialysis bag and immersed in deionized water. The deionized water was replaced every 8 h until the pH value of the immersion liquid was neutral, thereby obtaining hemostatic aerogel 2-2; wherein the heating temperature was 80°C and the time was 3 h.

[0104] The final hemostatic aerogel 2-2 has spiral pores; the porosity of the hemostatic aerogel 2-2 is 66%, and the pore size is 2 to 8 μm; the BCI value of the hemostatic aerogel 2-2 is 3%, the water absorption rate is 1875%, and the blood absorption rate is 1287%; the average hemostatic time of the hemostatic aerogel 2-2 in the rat tail amputation wound model is 115 s and the average blood loss is 771 mg.

[0105] Example 6

[0106] A method for preparing a hemostatic aerogel, the specific steps are as follows:

[0107] (1) Preparation of raw materials;

[0108] Hydrophilic fiber material: cellulose acetate fiber, water contact angle of 30° to 75°, shear stiffness of 10 to 20, aspect ratio of 40 to 60;

[0109] Hydrophobic fiber material: polycaprolactone fiber, water contact angle of 100° to 130°, shear stiffness of 0.1 to 0.5, aspect ratio of 40 to 80;

[0110] water;

[0111] Cross-linking agent aqueous solution: the cross-linking agent is tannic acid (CAS No. 1401-55-4);

[0112] (2) a hydrophilic fiber material and a hydrophobic fiber material in a mass ratio of 1.5:1 are dispersed in water, and after shearing for 8 minutes by a shearing machine, a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 3 minutes to obtain a fiber suspension; wherein the shearing rate of the shearing machine is 15000 rpm; the content of the hydrophilic fiber material in the fiber suspension is 0.6 wt %, and the content of the crosslinking agent is 0.3 wt %;

[0113] (3) The fiber suspension was allowed to stand at -196°C (supercooling degree was 8°C) for 0.2 h, freeze-dried (temperature was -60°C, pressure was 40 Pa, and time was 48 h), and then heated to induce cross-linking to obtain hemostatic aerogel 3; wherein the heating temperature was 40°C and the time was 4 h.

[0114] The final hemostatic aerogel 3 has spiral pores; the porosity of the hemostatic aerogel 3 is 84%, and the pore size is 10-30 μm; the BCI value of the hemostatic aerogel is 1.4%, the water absorption rate is 2519%, and the blood absorption rate is 1708%; the average hemostatic time of the hemostatic aerogel 3 in the rat tail amputation wound model is 75 s and the average blood loss is 617 mg.

[0115] Under the same test conditions, the BCI values ​​of hemostatic aerogel 1-1, hemostatic aerogel 1-2, hemostatic aerogel 1-3, hemostatic aerogel 2-1, hemostatic aerogel 2-2, hemostatic aerogel 3, hemostatic cotton ball, hemostatic gelatin sponge and hemostatic gauze are compared as shown in the figure below. Figure 3 As shown in the water absorption comparison chart Figure 4 As shown in the figure, the blood absorption rate comparison is as follows Figure 5 As shown; under the same test conditions, the comparison diagrams of the average hemostatic time and average blood loss of hemostatic aerogel 1-1, hemostatic aerogel 1-2, hemostatic aerogel 1-3, hemostatic aerogel 2-1, hemostatic aerogel 2-2, hemostatic aerogel 3, hemostatic cotton balls, hemostatic gelatin sponges and hemostatic gauze in the rat tail amputation wound model are shown as follows: Figure 6 , Figure 7 shown.

Claims

1. A method for preparing a hemostatic aerogel, characterized in that: After preparing a fiber suspension in which a hydrophilic fiber material and a hydrophobic fiber material are dispersed and a crosslinking agent is dissolved by shearing with a shearing machine, the fiber suspension is frozen until it is completely frozen, and after freeze-drying, cross-linking is initiated, or further post-processing is performed to obtain a hemostatic aerogel; The water contact angle of the hydrophilic fiber material is 30° to 80°, the shear stiffness is 10 to 20, and the aspect ratio is ≥40; the water contact angle of the hydrophobic fiber material is 100° to 140°, the shear stiffness is 0.1 to 0.5, and the aspect ratio is ≥40; the mass ratio of the hydrophilic fiber material to the hydrophobic fiber material is 1 to 2:1; the shear rate of the shearing machine is 10000 to 15000 rpm; the supercooling degree during freezing is ≥5.5°C.

2. The method for preparing a hemostatic aerogel according to claim 1, characterized in that: The preparation process of the fiber suspension is as follows: the hydrophilic fiber material and the hydrophobic fiber material are dispersed in water, sheared by a shearing machine for 5 to 8 minutes, and then a crosslinking agent aqueous solution is added thereto, and the shearing is continued for 3 to 5 minutes to obtain the fiber suspension.

3. The method for preparing a hemostatic aerogel according to claim 1, characterized in that: The hydrophilic fiber material is cellulose fiber or cellulose derivative fiber; the hydrophobic fiber material is thermoplastic polyurethane fiber, polylactic acid fiber or polycaprolactone fiber; and the crosslinking agent in the crosslinking agent aqueous solution is a crosslinking agent containing epoxy group, amino group or carboxyl group.

4. The method for preparing a hemostatic aerogel according to claim 3, characterized in that: In the fiber suspension, the content of the hydrophilic fiber material is 0.5-0.67wt%.

5. The method for preparing a hemostatic aerogel according to claim 3, characterized in that: In the fiber suspension, the content of the crosslinking agent is 0.25-0.5wt%.

6. The method for preparing a hemostatic aerogel according to claim 3, characterized in that: Freezing the fiber suspension until it is completely frozen means leaving the fiber suspension at -50 to -196°C for 0.2 to 8 hours.

7. The method for preparing a hemostatic aerogel according to claim 3, characterized in that: The cross-linking is initiated by heating at a temperature of 40 to 120° C. for a time of 2 to 4 hours.

8. A hemostatic aerogel prepared by the method for preparing a hemostatic aerogel according to any one of claims 1 to 7, characterized in that: With spiral hole.

9. The hemostatic aerogel according to claim 8, characterized in that: The porosity of the hemostatic aerogel is 64-92%, and the pore size is 2-30 μm.

10. The hemostatic aerogel according to claim 8, characterized in that: The BCI value of the hemostatic aerogel is 0.6-3%, the water absorption rate is 1328-4197%, the blood absorption rate is 885-1708%, the average hemostasis time in the rat tail amputation wound model is 30-120s and the average blood loss is 250-882mg.

Citation Information

Cited By

  • Asymmetric short fiber aerogel stent loaded with magnesium oxide as well as preparation method and application of asymmetric short fiber aerogel stent

    CN120754304A

  • An airway hemostatic aerogel and method of making same

    CN122912173A