Preparation method of bulk phase hydrocracking catalyst

By adopting a stepped pore size distribution and adding β molecular sieve slurry in stages in the preparation of hydrocracking catalysts, the problems of insufficient active metal loading and poor nitrogen resistance of existing catalysts are solved, and efficient polycyclic aromatic hydrocarbon conversion and nitrogen resistance are achieved. Improved performance to meet industrial grade special oil standards.

CN118767975AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310368844.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Existing hydrocracking catalysts have insufficient active metal loading under high pressure, small pore volume and specific surface area, and cannot meet the polycyclic aromatic hydrocarbon conversion requirements of industrial white oil and transformer oil. They also have poor nitrogen tolerance, which affects the conversion effect of isomers and aromatic hydrocarbons.

Method used

A bulk phase hydrocracking catalyst preparation method is adopted, by adding deionized water and phosphate ester to the reaction tank, passing in CO2 to perform a gel-forming reaction, then adding a solution containing Ni and sodium metaaluminate, and adding β molecular sieve slurry in batches , aged and dried, and finally calcined to form a catalyst with stepped pore size distribution and highly active metal oxide particles.

Benefits of technology

It improves the active metal utilization rate and pore volume of the catalyst, enhances the synergistic effect of acidity and hydrogenation components, improves the nitrogen resistance performance and aromatic hydrocarbon conversion ability of the catalyst, meets the standards of industrial-grade special oil, and reduces operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004167945170000201
    Figure BDA0004167945170000201
  • Figure BDA0004167945170000211
    Figure BDA0004167945170000211
  • Figure BDA0004167945170000212
    Figure BDA0004167945170000212
Patent Text Reader

Abstract

The invention discloses a bulk phase hydrocracking catalyst preparation method, which comprises: (1) adding deionized water and phosphate into a reaction tank, continuously introducing CO2, and carrying out a gel forming reaction on a solution containing W and Mo and a sodium metaaluminate solution A to obtain a material A; (2) adding a Ni-containing solution and a precipitant aqueous solution into the material A, carrying out reaction and aging treatment, adding a sodium metaaluminate solution B and beta molecular sieve slurry in n times in the aging process, and filtering the obtained slurry to obtain a material B; and (3) carrying out primary drying, grinding, molding and washing on the material B obtained in the step (2), and then carrying out secondary drying and roasting to obtain the bulk phase hydrocracking catalyst. The catalyst prepared by the invention has excellent isomerization performance and aromatic hydrocarbon conversion capability, and is suitable for being applied to a hydrocracking process for producing special oil and lubricant base oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum refining, and in particular relates to a method for preparing a bulk hydrocracking catalyst. Background Art

[0002] The hydrocracking diesel fraction has the characteristics of water white color, low impurity content, and high saturated hydrocarbon content. It can be blended to produce various white oils, anti-rust oils, transformer oils, aluminum cold rolling oils, etc. The hydrocracking tail oil fraction is suitable for lubricating oil base oil. Depending on the brand, the pour point index of industrial white oil is between -3 and -9 ° C, and the aromatic mass content is required to be no more than 5%. According to the lowest cold state operation temperature in actual application, the product pour point index range of transformer oil is between -10 ° C and -50 ° C, and the polycyclic aromatic hydrocarbon content is required to be less than 3%. According to the product indicators of special oils, the hydrocracking catalyst needs to take into account both high isomerization performance and high aromatic conversion ability, which requires the acidic components and hydrogenation active metal components in the catalyst to have good synergistic effects.

[0003] At present, the acidic components commonly used in hydrocracking are Y molecular sieve, β molecular sieve, and ZSM-5 molecular sieve. Among them, β molecular sieve has the best isomerization performance and can meet the pour point index requirements of industrial white oil. However, it is difficult for conventional supported hydrogenation catalysts and bulk catalysts prepared by existing technologies to meet the requirements for the content of polycyclic aromatic hydrocarbons in industrial white oil.

[0004] Hydrocracking is carried out under high pressure, and hydrocarbon molecules and hydrogen react on the catalyst surface to crack and hydrogenate to generate lighter molecules. Hydrodesulfurization, denitrogenation and hydrogenation of unsaturated hydrocarbons also occur. Traditional supported hydrocracking catalysts are limited by the pore structure of the carrier, and the active metal loading is generally not more than 30wt%. The hydrogenation activity of the catalyst is far from reaching the aromatic conversion activity when producing high value-added special oil products. The bulk hydrocracking catalyst prepared by coprecipitation has a high active metal content, but the oxide particles generated during the coprecipitation reaction are of different sizes, the pore volume and specific surface area of ​​the catalyst are small, and the active metal utilization rate is low. The molecular sieve is mostly added after the active metal precipitation is generated, and the pores of the oxide particles formed before and the molecular sieve pores cannot be interconnected, which reduces the mutual coordination between the acidic component and the hydrogenation component and the diffusion performance of the catalyst, thereby weakening the hydrocracking activity of the bulk catalyst. Therefore, the bulk catalyst produced by the existing technology still cannot meet the hydrogenation activity requirements required for the production of high value-added special oil products. At the same time, the nitrogen resistance of the hydrocracking catalyst also affects its isomerization and aromatic conversion effects. The nitrogen-containing compounds in the hydrocracking feedstock have different degrees of poisoning (shielding) effects on the acidic centers of the hydrocracking catalyst. The hydrocracking catalyst has good nitrogen resistance, which can improve the catalyst's raw material adaptability and extend the operating cycle of the industrial unit.

[0005] CN106179462A discloses a hydrocracking catalyst and a preparation method thereof, wherein the method first adopts a positive addition method to prepare a precipitate slurry I containing Ni and Al components, and then adopts a parallel flow method to prepare a precipitate slurry II containing W, Si and Al components, and the two precipitate slurries are mixed evenly, aged and filtered, and the obtained material is mixed with urea, subjected to hydrothermal treatment in water vapor, and then a Y-type molecular sieve suspension is added. The catalyst oxide obtained by the method is of different sizes, and the surface active metals are excessively accumulated after the hydrothermal treatment, and the utilization rate of the surface active metals is not improved. At the same time, after the molecular sieve is added, the interaction between the catalyst acid component and the hydrogenation component is greatly reduced.

[0006] CN103055923A discloses a method for preparing a hydrocracking catalyst. The method is as follows: prepare an acidic mixed solution A containing hydrogenation active metals and silicon, prepare an alkaline solution B of sodium metaaluminate, then add the acidic mixed solution A, alkaline solution B and gas CO2 to a reaction tank filled with clean water to form a gel, add a suspension of Y-type molecular sieves to mix evenly, filter, dry, shape, and then wash, dry, and roast to obtain a hydrocracking catalyst. This method can increase the pore volume and specific surface area of ​​the catalyst, but this method only relies on the carbonate generated in the precipitation to release gas during roasting to increase the pore volume, specific surface area and improve the dispersion of active catalyst metals. At the same time, it is easy to cause the active metals in the catalyst to aggregate.

[0007] CN110038617A discloses a hydrocracking catalyst and its preparation method. The hydrocracking catalyst is a bulk catalyst, which is prepared by firstly subjecting a mixed solution A containing Ni, W and Al components to a precipitant in parallel to a gelling reaction, subjecting the obtained slurry to preliminary aging, then subjecting a mixed solution B containing W, Si and Al components to a precipitant in parallel to the aged slurry to a reaction, then subjecting the precipitant to the addition of a molecular sieve suspension to aging, and then subjecting the catalyst to post-treatment to prepare a hydrocracking catalyst. The catalyst has a small specific surface area and pore volume, and its hydrogenation activity cannot meet the standards of industrial-grade white oil products.

[0008] CN106513006A discloses a method for preparing a bulk hydrogenation refining catalyst, which comprises: mixing and pre-dispersing a Ni-containing compound with deionized water under an ultrasonic environment, then adding a Mo-containing compound to form a Ni-Mo fine grain structure, then adding a W-containing compound and a complexing agent for hydrothermal reaction, and then kneading and extruding the obtained active component powder with aluminum hydroxide dry glue, and drying and calcining to obtain a catalyst. The catalyst prepared by the method of the present invention has uniform dispersion between different active phase grains, the active metal of the bulk catalyst is not fully utilized, the amount of active metal in the surface phase is small, and the hydrogenation performance is not fully improved.

[0009] The hydrogenation activity of catalysts prepared by existing technologies cannot meet the production of industrial white oil. Therefore, improving the utilization rate of active metals in bulk catalysts and improving the coordination between hydrogenation components and acidic components are the key to ensuring that bulk hydrocracking catalysts meet the production of industrial white oil. Summary of the invention

[0010] In view of the deficiencies of the prior art, the present invention provides a method for preparing a bulk hydrocracking catalyst. The catalyst prepared by the method has a stepped pore size distribution, a large surface active site density, a small active metal oxide particle size and a uniform distribution, a good synergistic effect between the hydrogenation active component and the acid component, and good nitrogen resistance. The catalyst prepared by the present invention also has excellent isomerization performance and aromatic conversion ability, and is suitable for use in the hydrocracking process for producing specialty oils and lubricating oil base oils.

[0011] The method for preparing the bulk hydrocracking catalyst of the present invention comprises:

[0012] (1) adding deionized water and phosphate into a reaction tank, continuously introducing CO2, and adding a solution containing W and Mo and a sodium aluminate solution A into the reaction tank in parallel to perform a gelling reaction to obtain material A;

[0013] (2) adding the Ni-containing solution and the precipitant aqueous solution to the material A obtained in step (1) to react, and then aging the material A. During the aging process, sodium aluminate solution B and β molecular sieve slurry are added n times to obtain a slurry which is filtered to obtain material B. The sodium aluminate solution B and β molecular sieve slurry are added n times in the following manner: each time, 1 / n volume of sodium aluminate solution B is first added, and then 1 / n volume of β molecular sieve slurry is added, and the process is performed n times in total, where n is an integer between 2 and 8.

[0014] (3) The material B obtained in step (2) is first dried, rolled, formed, washed, and then second dried and calcined to obtain a bulk hydrocracking catalyst.

[0015] In the method of the present invention, the phosphate ester described in step (1) is one or more of octadecyl ether phosphate (O-5P), alkylphenol ether phosphate (TXP-4, TXP-10), isomeric tridecanol ether phosphate (E-1310P), lauryl alcohol ether phosphate (MOA-3P, MOA-9P), castor oil phosphate, octadecyl phosphate, and lauryl phosphate, preferably one or more of alkylphenol ether phosphate (TXP-4, TXP-10), isomeric tridecanol ether phosphate (E-1310P), lauryl alcohol ether phosphate (MOA-3P, MOA-9P), and castor oil phosphate. The molar ratio of the phosphate ester to Al in the sodium aluminate solution in step (1) is 0.2:1 to 2.0:1, preferably 0.3:1 to 1.8:1.

[0016] In the method of the present invention, the concentration of the added CO2 gas in step (1) is 40v% to 70v%; the flow rate of the CO2 gas is 30 to 120mL / min, and the introduction of the CO2 gas is stopped after the gelling reaction is completed.

[0017] In the method of the present invention, in the W and Mo-containing solution described in step (1), the weight concentration of W calculated as WO3 is 5 to 120 g / L, preferably 10 to 110 g / L, and the weight concentration of Mo calculated as MoO3 is 5 to 110 g / L, preferably 10 to 100 g / L; wherein, when preparing the W and Mo-containing solution, the tungsten source generally used is ammonium metatungstate, and the molybdenum source is ammonium molybdate.

[0018] In the method of the present invention, the concentration of the sodium aluminate solution A in step (1) is 5 to 90 g / L, preferably 8 to 80 g / L, in terms of Al2O3 concentration.

[0019] In the method of the present invention, the conditions for the gelling reaction in step (1) are: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value of the co-current reaction is controlled at 5 to 6, and the reaction time is 0.1 to 1.0 hour.

[0020] In the method of the present invention, in the Ni-containing solution described in step (2), the weight concentration of Ni in terms of NiO is 5 to 130 g / L, preferably 10 to 115 g / L; when preparing the Ni-containing solution, the nickel source is generally one or more of nickel sulfate, nickel nitrate, and nickel chloride; in the sodium aluminate solution B, the weight concentration of Al in terms of Al2O3 is 5 to 70 g / L, preferably 8 to 60 g / L.

[0021] In the method of the present invention, in step (2), the sodium aluminate solution B is preferably divided into n equal parts by volume, wherein n is an integer of 2 to 8; and the β molecular sieve slurry is preferably divided into n equal parts by volume, wherein n is an integer of 2 to 8.

[0022] In the method of the present invention, the precipitating agents described in step (2) are all alkaline precipitating agents, selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium hydroxide, potassium carbonate or potassium bicarbonate, preferably ammonia water and sodium hydroxide. The concentration of the precipitating agent aqueous solution is adjusted according to actual needs, such as the concentration of the sodium hydroxide solution is 7wt% to 20wt%.

[0023] In the method of the present invention, the reaction conditions of step (2) are as follows: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value is controlled at 8.0 to 12.0 at the end, and the reaction time is 0.5 to 2.5 hours; preferably, the reaction temperature of step (2) is the same as the reaction temperature of step (1).

[0024] In the method of the present invention, the aging treatment conditions described in step (2) are: the aging temperature is 60-98°C, preferably 65-92°C. The aging process is carried out in the following manner: n times of three-stage decreasing pH aging are carried out, and each time of the three-stage decreasing pH aging, when adjusting the pH value in the first stage, 1 / n volume of sodium aluminate solution B is used for adjustment, and 1 / n volume of β molecular sieve slurry is added after adjustment; wherein the three-stage decreasing pH aging is: in the first stage, the pH value is 11.0-13.5, and the aging time is 0.05-0.5 hours; in the second stage, the pH value is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; in the third stage, the pH value is adjusted to 4.5-6.2, and the aging time is 0.05-0.5 hours.

[0025] Among them, except for the use of sodium aluminate solution B in the first stage pH value adjustment during the aging process, the acids and alkalis used for adjusting the pH value can be inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements. The inorganic acid can be hydrochloric acid and acetic acid, and the inorganic alkali can be one or more of sodium carbonate, sodium bicarbonate, and sodium hydroxide. The concentration and dosage of the acid and alkali solutions can be adjusted according to the actual preparation needs.

[0026] In the method of the present invention, in step (2), the Al added to the sodium aluminate solution B accounts for 5% to 55% of the total Al in the obtained catalyst calculated as Al2O3, preferably 6% to 50%.

[0027] In the method of the present invention, the beta molecular sieve described in step (2) has the following properties: a molar ratio of silicon oxide to aluminum oxide of 30 to 90; a specific surface area of ​​430 to 780 m 2 / g, preferably 400-700m 2 / g; pore volume is 0.30~0.90cm 3 / g, preferably 0.35 to 0.85 cm 3 / g; the infrared acid content is 0.10-0.45mmol / g, preferably 0.18-0.40mmol / g; the beta molecular sieve slurry is a uniform mixture of beta molecular sieve and deionized water, with a solid-liquid mass ratio of 1:1.1-1:5.5, preferably 1:1.3-1:5.0.

[0028] In the method of the present invention, the first drying, molding and washing described in step (3) can be carried out by conventional methods in the art. The first drying conditions are as follows: drying at 40-150°C for 1-48 hours, preferably drying at 50-120°C for 4-36 hours. During the molding process, conventional molding aids, such as one or more of peptizing agents, extrusion aids, etc., can be added as needed. The peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the extrusion aid refers to a substance that is conducive to extrusion molding, such as one or more of sesbania powder, carbon black, graphite powder, citric acid, etc., and the amount of the extrusion aid accounts for 1wt% to 10wt% of the total material dry basis. Washing is generally carried out with deionized water or a solution containing decomposable salts (such as ammonium acetate, ammonium chloride, ammonium nitrate, etc.) until neutral.

[0029] The second drying process described in step (3) is:

[0030] a. First, dry the material at 60-100°C for 1.0-8.5 hours, preferably at 70-90°C for 2.0-8.0 hours;

[0031] b. Evenly spray water on the material obtained in step a, the volume ratio of water to dry material is 1:4 to 4:1, and then dry at a temperature of 150 to 280° C., preferably 150 to 250° C., for 0.5 to 4.0 hours, preferably 0.6 to 3.5 hours;

[0032] c. Repeat step b 2 to 9 times, preferably 3 to 8 times;

[0033] Among them, the volume ratio of the first added water volume to the dry material is greater than 1:1, and the volume ratio of the last added water volume to the dry material is less than 1:1. Furthermore, the volume ratio of the added water volume to the dry material gradually decreases with the increase in the number of repetitions.

[0034] Furthermore, the total drying time used for the second drying is preferably 5 to 40 hours, and more preferably 7 to 38 hours.

[0035] In the method of the present invention, the calcination conditions in step (3) are as follows: calcination at 350-650° C. for 1-24 hours, preferably calcination at 400-600° C. for 2-12 hours.

[0036] The present invention also provides a hydrocracking catalyst which is a bulk hydrocracking catalyst. The hydrocracking catalyst comprises a hydrogenation active metal component, amorphous alumina and a beta molecular sieve. The catalyst particles comprise an outer surface layer, an intermediate layer and a central core, and the average pore diameter decreases in a gradient, that is, the average pore diameter of the outer surface layer is greater than the average pore diameter of the intermediate layer, and the average pore diameter of the intermediate layer is greater than the average pore diameter of the central core. The average pore diameter of the outer surface layer is 11-19 nm, the average pore diameter of the intermediate layer is 7-11 nm, and the average pore diameter of the central core is 3-7 nm, wherein on the cross section of the catalyst particle, the length from the outermost edge to the center point is R; the thickness of the outer surface layer is 0.2R-0.4R, the thickness of the intermediate layer is 0.2R-0.5R, and the rest is the central core; the molar ratio of W / Mo is 1:5-21:1, preferably 1:3-19:1, and the molar ratio of Ni / (Mo+W) is 1:14-16:1, preferably 1:12-14:1. The ratio of the sum of the weight contents of the surface active metal components WO3 and NiO to the sum of the weight contents of the bulk active metal components WO3 and NiO is 2.8:1 to 6.5:1, preferably 3.4:1 to 6.2:1, and the ratio of the sum of the weight contents of the surface active metal components MoO3 and NiO to the sum of the weight contents of the bulk active metal components MoO3 and NiO is 2.0:1 to 5.5:1, preferably 2.2:1 to 5.2:1. The catalyst of the present invention is in the form of (solid) particles, and the average pore diameter is from large to small from the outer surface layer of the catalyst to the central core.

[0037] In the catalyst of the present invention, the average particle size of the active metal oxide particles of tungsten, molybdenum and nickel is 10 to 14 nm. Preferably, the particle size distribution of the oxide particles is as follows: the number of particles with a particle size less than 10 nm accounts for 2% to 17% of the total number of particles, the number of particles with a particle size of 10 nm to 14 nm accounts for 72% to 90% of the total number of particles, and the number of particles with a particle size greater than 14 nm accounts for 3% to 19% of the total number of particles.

[0038] The hydrocracking catalyst is in the form of (solid) particles and can be prepared by conventional molding methods. The shape can be various shapes conventionally used for hydrocracking catalysts, such as cylindrical, spherical, etc. The spherical shape can be spherical, ellipsoidal, etc., and the columnar shape can be cylindrical, square columnar, or a cross-sectional columnar shape of a special shape (such as a clover, a four-leaf clover, etc.). The particle size of the catalyst particles is 1 to 10 mm. Generally, when it is cylindrical, the length can be 2 to 10 mm, and the particle size can be 1 to 6 mm. Generally, when it is spherical, the particle size is 2 to 10 mm.

[0039] The hydrocracking catalyst of the present invention can be used in the hydrocracking process of base oil for producing special oil and lubricating oil, and is particularly suitable for the hydrocracking process of base oil raw materials for producing transformer oil, white oil and high viscosity index lubricating oil.

[0040] The hydrocracking catalyst of the present invention is applicable to a wide range of heavy raw materials, including one or more of various hydrocarbon oils such as vacuum gas oil, coking gas oil, deasphalted oil, thermal cracking gas oil, catalytic cracking gas oil, catalytic cracking circulating oil, etc., usually containing hydrocarbons with a boiling point of 250-550°C, and a nitrogen content of 300-2500 μg / g. After the hydrocracking pretreatment process, the nitrogen content in the feed of the hydrocracking catalyst of the present invention is less than 150 μg / g, that is, the nitrogen content in the feed of the hydrocracking catalyst reaction section is less than 150 μg / g, further more than 10 μg / g, even more than 50 μg / g. The hydrocracking catalyst of the present invention still has high activity, stability and good product quality under high nitrogen content feed conditions (less than 150 μg / g).

[0041] Compared with the prior art, the present invention has the following advantages:

[0042] 1. The method of the present invention controls the preparation steps and preparation conditions comprehensively, so that the oxide particles have a small particle size and are evenly distributed, and can fully contact with the molecular sieve. At the same time, the pore volume and pore size of the catalyst surface phase are increased, which increases the probability of the active component carrier pores and the molecular sieve pores being interconnected, and improves the diffusion performance of the catalyst and the interaction between the hydrogenation component and the acidic component. The catalyst surface phase has a high hydrogenation active site and a stepped pore distribution, which can hydrogenate more and faster organic nitrogen-containing compounds that have a large poisoning effect on the acid center of the catalyst, play a protective role on the acid center of the catalyst, improve the nitrogen resistance of the hydrocracking catalyst, and improve the properties of the hydrocracking product.

[0043] 2. During the gelation process of step (1) of the method of the present invention, when CO2 gas is introduced, the gas concentration and flow rate are controlled to obtain ideal microbubbles in the reaction liquid, which are small in size, suspended in the water and free, and constantly perform irregular collisions. Under the combined effect of the phosphate ester and the microbubbles in the reaction liquid, the particle size of the metal oxide in the catalyst is small, which helps to improve the dispersibility of the active metal, reduce the probability of micropores, and increase the pore volume and specific surface area of ​​the bulk catalyst.

[0044] 3. In step (2) of the present invention, a solution containing Ni is added dropwise to the W, Mo, and Al precipitation slurry with good dispersibility and small particle size prepared in step (1). The specific addition sequence, corresponding pH value control, and active metal precipitation sequence optimize the pore size distribution and active metal dispersibility of the resulting catalyst, and the active metal content in the surface phase is significantly increased. This is beneficial to improving the hydrogenation saturation activity of the W-Ni combination and the hydrogenation denitrification activity of the Mo-Ni combination. As the surface metal content increases, the synergistic effect of the acidic component and the hydrogenation component is further enhanced.

[0045] 4. In the present invention, the pH value is swung during aging and sodium aluminate solution is added in batches. The pH value swing is used to dissolve the amorphous oxide in the oxide particles. The addition of sodium aluminate solution re-modifies the size of the oxide particles. With each simultaneous addition of molecular sieves, the metal oxide particles are in better contact with the molecular sieves, thereby promoting the synergistic effect of the acidic component and the hydrogenation component.

[0046] 5. When the second drying method after forming is adopted in the method of the present invention, the pore distribution of the catalyst particles is such that the average pore diameter decreases from large to small from the outer surface layer of the catalyst to the central core, presenting a stepped pore size distribution. This can reduce the influence of the diffusion effect of reactants such as macromolecules with larger molecular diameters when entering and exiting the catalyst pores, which is beneficial to improving the diffusion performance of the catalyst for macromolecules, and is more conducive to the hydrogenation of reactants such as macromolecules with larger diameters by active metals such as tungsten, nickel, and molybdenum in the catalyst surface phase.

[0047] The hydrocracking catalyst obtained by the preparation method of the present invention has high aromatic saturation reaction performance, and the catalyst has both high isomerization performance and high aromatic conversion capacity. When used in the process of producing special oils by hydrocracking, the aromatic content and pour point of the hydrocracking diesel fraction product can meet the requirements of the industrial-grade special oil base oil standard, and can reach the standard of the industrial-grade special oil base oil without further deep processing, thereby reducing operating costs, increasing product added value, and creating greater economic benefits. The hydrocracking catalyst of the present invention still has good stability and good product quality under high nitrogen content feed conditions. DETAILED DESCRIPTION

[0048] In the present invention, the specific surface area and pore volume are measured by low-temperature liquid nitrogen adsorption method, and the mechanical strength is measured by lateral pressure method.

[0049] In the present invention, the active metal content of the catalyst surface phase is measured by X-ray photoelectron spectroscopy (XPS), and the active metal content of the catalyst bulk phase is measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES).

[0050] In the present invention, wt% refers to mass fraction, and v% refers to volume fraction.

[0051] In the present invention, the average particle size (D50 particle size) and particle size distribution of the active metal oxide particles are measured using a nanoparticle size and Zeta potential analyzer (Zetasizer Nano ZS).

[0052] In the present invention, the "cross-section of a catalyst particle" refers to the entire surface exposed after cutting through the geometric center of its shape along the direction of the smallest dimension of a catalyst particle. For example, when the catalyst particle is spherical, the cross-section refers to the entire surface exposed after cutting through the center of the sphere along the radius or short axis direction of the sphere. Alternatively, when the catalyst particle is columnar, the cross-section refers to the entire surface exposed after cutting through the center point of the length dimension perpendicular to the length dimension of the column. The periphery of the exposed surface is referred to as the outermost edge of the cross-section, and the geometric center (such as the aforementioned center of the sphere or the center point of the length dimension) is referred to as the center point on the cross-section.

[0053] In the present invention, the method for determining the average pore diameter of different layers from the outer surface layer to the central core of the catalyst particles is as follows: first, the pore volume, specific surface area and average pore diameter of the sample are determined by the low temperature nitrogen adsorption method (BET), and then a certain amount of the sample is taken and placed in a catalyst abrasion tester, and the sample is polished, and a certain amount of quartz sand is added to increase the wear rate. When the particle size of the sample is reduced to a certain extent after polishing, the weight loss of the sample is measured and its pore structure is measured again. From the relationship that the total pore volume and specific surface area of ​​the sample are equal to the sum of each part, the pore volume and specific surface area of ​​the polished part can be calculated, and 20-80 samples are measured at the same time to calculate the average pore diameter. In this way, the average pore diameter of different layers from the outer surface layer to the central core is determined.

[0054] In the present invention, the properties of the β molecular sieve used are shown in Table 7, and the properties of the Y molecular sieve are shown in Table 8.

[0055] Example 1

[0056] Ammonium metatungstate and ammonium molybdate are added to dissolution tank 1 filled with deionized water to prepare solutions containing W and Mo. The weight concentration of W in the solution containing W and Mo is 68g / L in terms of WO3, and the weight concentration of Mo in terms of MoO3 is 32g / L. Nickel chloride is added to dissolution tank 2 filled with deionized water to prepare a Ni-containing solution. The weight concentration of Ni in the Ni-containing solution is 52g / L in terms of NiO. Al in sodium metaaluminate solution B accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrocracking catalyst, and it is divided into 5 equal parts by volume. Beta molecular sieve slurry is prepared at a solid-liquid ratio of 1:3, and it is divided into 5 equal parts by volume. Deionized water and isomeric tridecanol ether phosphate (E-1310P) with a molar ratio of 0.9 to the total number of Al atoms in sodium aluminate solution A are added to the reaction tank, and CO2 gas with a concentration of 52v% is introduced into the reaction tank solution at a flow rate of 80ml / min. A solution containing W and Mo and a sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 is 8.4 g / L) are added to a reaction tank in parallel to carry out a gelling reaction. The reaction pH is controlled at 5.4 and the reaction temperature is 62°C. After the reaction for 0.8 hour, a Ni-containing solution and a sodium hydroxide solution (weight concentration is 10%) are simultaneously added dropwise to the reaction slurry. The reaction temperature remains unchanged and the reaction time is 1.0 hour. At the end of the reaction, the pH is controlled at 8.8. After the reaction is completed, the introduction of CO2 gas is stopped to generate a precipitate slurry containing nickel, molybdenum, tungsten, aluminum and phosphorus. The resulting slurry is aged at an aging temperature of 78°C. During aging, an equal portion of sodium aluminate solution B is first added to control the pH to 13.1, and an equal portion of β molecular sieve slurry is added. After aging for 0.2 hour, the aging pH is controlled at 9.6. After aging for 0.2 hour, the pH is then controlled to 5.5 for 0.15 hour. The above operation process is repeated 5 times to terminate the aging. The obtained slurry was filtered, and the filter cake was dried for the first time at 100°C for 9 hours, rolled, extruded and washed with deionized water at room temperature until neutral. Then the washed wet strips are dried in the following steps: first, the material is dried at 78°C for 7.5 hours, deionized water is evenly sprayed on the dried material, and then dried, and the evenly spraying deionized water and drying process are repeated 5 times, the volume ratio of deionized water to dry material spraying for the first time is 2.0:1, the drying temperature is 190°C, and the drying time is 2.0 hours, the volume ratio of deionized water to dry material spraying for the second time is 1.5:1, the drying temperature is 190°C, and the drying time is 2.2 hours, the volume ratio of deionized water to dry material spraying for the third time is 1:1, the drying temperature is 180°C, and the drying time is 1.8 hours, the volume ratio of deionized water to dry material spraying for the fourth time is 1:1.8, the drying temperature is 180°C, and the drying time is 1.8 hours, and the volume ratio of deionized water to dry material spraying for the fifth time is 1:2.3, the drying temperature is 200°C, and the drying time is 1.9 hours.The dried material was calcined at 540°C for 4 hours to obtain catalyst A. The composition and main properties of the catalyst are shown in Table 1.

[0057] Example 2

[0058] Ammonium metatungstate and ammonium molybdate are added to the dissolving tank 1 filled with deionized water to prepare a mixed solution containing W and Mo. The weight concentration of W in the solution containing W and Mo is 52g / L in terms of WO3, and the weight concentration of Mo in terms of MoO3 is 24g / L. Nickel chloride is added to the dissolving tank 2 filled with deionized water to prepare a Ni-containing solution. The weight concentration of Ni in the Ni-containing solution is 72g / L in terms of NiO. Al in the sodium aluminate solution B accounts for 35% of Al (in terms of Al2O3) in the obtained hydrocracking catalyst, and the solution is divided into 6 equal parts by volume. The beta molecular sieve slurry is prepared at a solid-liquid ratio of 1:3.2 and divided into 6 equal parts by volume. Deionized water and castor oil phosphate with a molar ratio of 0.9 to the total number of Al atoms in the sodium aluminate solution A are added to the reaction tank, and CO2 gas with a concentration of 57v% is introduced into the reaction tank solution, and the flow rate of CO2 gas is 70ml / min. A solution containing W and Mo and a sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 is 10.5 g / L) are added to a reaction tank in parallel to carry out a gelling reaction. The reaction pH is controlled at 5.2 and the reaction temperature is 55°C. After the reaction for 0.8 hour, a Ni-containing solution and a sodium hydroxide solution (weight concentration is 12%) are simultaneously added dropwise to the reaction slurry. The reaction temperature remains unchanged and the reaction time is 1.3 hours. At the end of the reaction, the pH is controlled at 9.5. After the reaction, the introduction of CO2 gas is stopped to generate a precipitate slurry containing nickel, molybdenum, tungsten, aluminum and phosphorus. The resulting slurry is aged at an aging temperature of 80°C. During aging, an equal portion of sodium aluminate solution B is first added to control the pH to 13.0. An equal portion of β molecular sieve slurry is added. After aging for 0.15 hour, the aging pH is controlled at 10.1. After aging for 0.15 hour, the pH is then controlled to 4.8 for 0.2 hour. The above operation process is repeated 6 times to terminate the aging. The aged slurry was filtered, and the filter cake was dried for the first time at 90°C for 8 hours, rolled, extruded and washed with deionized water at room temperature until neutral.The washed wet strips were then dried for a second time in the following steps: first, the material was dried at 80°C for 7.2 hours, deionized water was sprayed evenly on the dried material, and then dried, and the uniform spraying of deionized water and the drying process were repeated 6 times, the first spraying of deionized water and the dried material volume ratio was 2.2:1, the drying temperature was 210°C, and the drying time was 2.2 hours, the second spraying of deionized water and the dried material volume ratio was 1.5:1, the drying temperature was 200°C, and the drying time was 2.0 hours, and the third spraying of deionized water and the dried material was 2.2:1. The volume ratio is 1:1.0, the drying temperature is 180℃, the drying time is 1.8 hours, the volume ratio of the fourth spraying deionized water to the dry material is 1:1.5, the drying temperature is 190℃, the drying time is 1.8 hours, the volume ratio of the fifth spraying deionized water to the dry material is 1:1.9, the drying temperature is 170℃, the drying time is 1.7 hours, the volume ratio of the sixth spraying deionized water to the dry material is 1:2.3, the drying temperature is 180℃, the drying time is 1.8 hours, and the dried material is calcined at 530℃ for 5 hours to obtain catalyst B. The catalyst composition and main properties are shown in Table 1.

[0059] Example 3

[0060] Ammonium metatungstate and ammonium molybdate are added to the dissolution tank 1 filled with deionized water to prepare W and Mo solutions. The weight concentration of W in the W and Mo solutions is 60g / L as WO3, and the weight concentration of Mo in MoO3 is 28g / L. Nickel chloride is added to the dissolution tank 2 filled with deionized water to prepare a mixed Ni solution. The weight concentration of Ni in the Ni solution is 60g / L as NiO. Al in the sodium metaaluminate solution B accounts for 38% of Al (as Al2O3) in the obtained hydrocracking catalyst, and it is divided into 5 equal parts by volume. The β molecular sieve slurry is prepared at a solid-liquid ratio of 1:2.8 and divided into 5 equal parts by volume. Deionized water and lauryl ether phosphate (MOA-9P) with a molar ratio of 1.2 to the total number of Al atoms in sodium aluminate A were added into the reaction tank, and CO2 gas with a concentration of 56v% was introduced into the reaction tank solution at a flow rate of 75ml / min. A solution containing W and Mo and a sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 is 10g / L) are added to a reaction tank in parallel to carry out a gelling reaction. The reaction pH is controlled at 5.9 and the reaction temperature is 65°C. After the reaction for 0.9 hour, a Ni-containing solution and ammonia water (weight concentration is 11%) are simultaneously added dropwise to the reaction slurry. The reaction temperature remains unchanged and the reaction time is 1.5 hours. At the end of the reaction, the pH is controlled at 10.5. After the reaction is completed, the introduction of CO2 gas is stopped to generate a precipitate slurry containing nickel, molybdenum, tungsten, aluminum and phosphorus. The resulting slurry is aged at an aging temperature of 80°C. During aging, an equal portion of sodium aluminate solution B is first added to control the pH to 12.6. An equal portion of β molecular sieve slurry is added. After the aging time of 0.2 hour, the aging pH is controlled at 9.6. After the aging time of 0.15 hour, the pH is then controlled to 5.0. When the aging time is 0.15, the above operation process is repeated 5 times to terminate the aging. The aged slurry was filtered, and the filter cake was dried for the first time at 100°C for 9 hours, rolled, extruded and formed into strips, and washed with deionized water at room temperature until neutral.The washed wet strips were then dried for a second time in the following steps: first, the material was dried at 84°C for 7.0 hours, deionized water was sprayed evenly on the dried material, and then dried, and the uniform spraying of deionized water and drying process were repeated 6 times, the first spraying of deionized water and dry material volume ratio was 2.0:1, the drying temperature was 200°C, and the drying time was 2.2 hours, the second spraying of deionized water and dry material volume ratio was 1.5:1, the drying temperature was 180°C, and the drying time was 1.9 hours, and the third The volume ratio of deionized water to dry material sprayed for the first time was 1.1:1, the drying temperature was 180℃, and the drying time was 1.8 hours. The volume ratio of deionized water to dry material sprayed for the fourth time was 1:1.3, the drying temperature was 170℃, and the drying time was 1.7 hours. The volume ratio of deionized water to dry material sprayed for the fifth time was 1:1.8, the drying temperature was 180℃, and the drying time was 1.8 hours. The volume ratio of deionized water to dry material sprayed for the sixth time was 1:2.2, the drying temperature was 170℃, and the drying time was 2.1 hours. The dried material was calcined at 510℃ for 6 hours to obtain catalyst C. The catalyst composition and main properties are shown in Table 1.

[0061] Example 4

[0062] Ammonium metatungstate and ammonium molybdate are added to the dissolution tank 1 filled with deionized water to prepare W- and Mo-containing solutions. The weight concentration of W in the W- and Mo-containing solutions is 64 g / L as WO3, and the weight concentration of Mo in MoO3 is 40 g / L. Nickel chloride is added to the dissolution tank 2 filled with deionized water to prepare Ni-containing solution. The weight concentration of Ni in the Ni-containing solution is 40 g / L as NiO. Al in the sodium metaaluminate solution B accounts for 30% of Al (as Al2O3) in the obtained hydrocracking catalyst, and the solution is divided into 4 equal parts by volume. The beta molecular sieve slurry is prepared at a solid-liquid ratio of 1:4.0, and the solution is divided into 4 equal parts by volume. Deionized water and isomeric tridecanol ether phosphate (E-1310P) having a molar ratio of 1.1 to the total number of Al atoms in sodium aluminate A were added to the reaction tank, and CO2 gas with a concentration of 55v% was introduced into the reaction tank solution at a flow rate of 90ml / min. A solution containing W and Mo and a sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 is 12.6 g / L) are added to a reaction tank in parallel to carry out a gelling reaction. The reaction pH is controlled at 5.2 and the reaction temperature is 70°C. After the reaction for 0.7 hour, a Ni-containing solution and ammonia water (weight concentration is 12%) are simultaneously added dropwise to the reaction slurry. The reaction temperature remains unchanged and the reaction time is 1.6 hours. At the end of the reaction, the pH is controlled at 10.2. After the reaction, the introduction of CO2 gas is stopped to generate a precipitate slurry containing nickel, molybdenum, tungsten, aluminum and phosphorus. The resulting slurry is aged at an aging temperature of 75°C. During aging, an equal portion of sodium aluminate solution B is first added to control the pH to 12.8. An equal portion of β molecular sieve slurry is added. After the aging time of 0.16 hour, the aging pH is controlled at 9.6. After the aging time of 0.2 hour, the pH is then controlled to 5.4. The aging time is 0.20 hour. The above operation process is repeated 4 times to terminate the aging. The obtained slurry was filtered, and the filter cake was dried for the first time at 80°C for 12 hours, rolled, extruded and washed with deionized water at room temperature until neutral.The washed wet strips were then dried in the following steps: first, the material was dried at 75°C for 7.0 hours, deionized water was evenly sprayed on the dried material, and then dried, and the even spraying of deionized water and drying process were repeated 6 times, the first spraying of deionized water and dry material volume ratio was 2.3:1, the drying temperature was 220°C, and the drying time was 2.3 hours, the second spraying of deionized water and dry material volume ratio was 1.8:1, the drying temperature was 180°C, and the drying time was 2.0 hours, and the third spraying of deionized water and dry material volume ratio was 1.8:1, the drying temperature was 180°C, and the drying time was 2.0 hours. The volume ratio of the fourth spraying deionized water to the dried material was 1:1.4, the drying temperature was 170°C, the drying time was 1.8 hours, the volume ratio of the fifth spraying deionized water to the dried material was 1:1.8, the drying temperature was 180°C, the drying time was 1.8 hours, the volume ratio of the sixth spraying deionized water to the dried material was 1:2.3, the drying temperature was 170°C, the drying time was 1.8 hours, and the dried material was calcined at 530°C for 5 hours to obtain catalyst D. The catalyst composition and main properties are shown in Table 1.

[0063] Comparative Example 1

[0064] Reference catalyst E was prepared according to the method disclosed in CN101239324A. The components and active metal content were the same as those in Example 1. The molecular sieve was β molecular sieve. The specific steps were as follows: (1) nickel chloride, ammonium molybdate, and aluminum chloride solution were added to a dissolution tank filled with deionized water. The mass concentration of Ni in the solution was 52 g / L in terms of NiO, the mass concentration of Mo in terms of MoO3 was 32 g / L, and the mass concentration of Al in terms of Al2O3 was 22 g / L. 2000 mL of clean water was added for dilution; (2) ammonia water was added under stirring until the pH value was 5.2; (3) a sodium tungstate solution containing 68 g / L of WO3 was prepared. Add to the mixture under stirring; (4) Continue to add ammonia water until the pH value is 7.8; (5) The entire gelling process should be carried out at 62°C; (6) The mixture is aged at 78°C for 4 hours; before aging, the β molecular sieve used in the preparation method is added, and the β molecular sieve accounts for 13% of the total weight of the catalyst. The properties are shown in Table 4, and the aging is completed; (7) Filter, dry in an oven at 100°C for 9 hours, roll, and extrude into strips using a perforated plate with a diameter of 3 mm; wash with ammonium acetate solution with a pH value of 8.8 at room temperature; then dry in an oven at 80°C for 10 hours, and calcine at 540°C for 4 hours to obtain Catalyst E. The catalyst composition and properties are shown in Table 1.

[0065] Comparative Example 2

[0066] According to the preparation method disclosed in CN106179462A, a reference agent F having the same catalyst composition as Example 1 of the present invention was prepared, wherein the acidic component was β molecular sieve, and the specific process was as follows:

[0067] Nickel chloride and aluminum chloride solutions were dissolved in deionized water to prepare mixed solution A, wherein the weight concentration of NiO in mixed solution A was 52 g / L and the weight concentration of Al2O3 was 15.4 g / L. Ammonium metatungstate, ammonium molybdate and aluminum chloride solutions were dissolved in deionized water to prepare mixed solution B, wherein the weight concentration of WO3 in mixed solution B was 68 g / L, the weight concentration of MoO3 was 32 g / L and the weight concentration of Al2O3 was 6.6 g / L. Ammonia water with a concentration of 10% (weight) was added to solution A under stirring, the gelling temperature was maintained at 6.2°C, the pH value was controlled at 7.8 at the end, and the gelling time was controlled at 0.8 hours to generate nickel-aluminum precipitate slurry I. Deionized water is added to the reaction tank, and 10% (weight) ammonia water and solution B are added to the reaction tank in parallel, the gelling temperature is maintained at 62°C, the pH value is controlled at 7.8 during the parallel gelling reaction, and the gelling time is controlled at 1.0 hour to generate slurry II containing tungsten, molybdenum and aluminum precipitates. The above two precipitate-containing slurries are mixed and aged, the aging time is 4.0 hours, the aging temperature is 78°C, the pH value is controlled at 7.6, and then filtered. The filter cake is hydrothermally treated under water vapor containing urea. The conditions of the hydrothermal treatment are: the molar ratio of urea to the total amount of active metal atoms is 7:1, the temperature is 250°C, the pressure is 4.0MPa, and the treatment time is 3 hours. After the treatment, the filter cake is slurried, and the β molecular sieve suspension is stirred evenly in the mixture slurry, filtered, and the filter cake is dried at 100°C for 9 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. Then the washed wet strips are dried at 80°C for 10.0 hours. The dried material was calcined at 540°C for 4 hours to obtain Catalyst F. The composition, pore distribution and main properties of the catalyst are shown in Table 1.

[0068] Comparative Example 3

[0069] The same reference agent G as in Example 1 was prepared, except that the acidic component was Y molecular sieve. The catalyst composition and main properties are shown in Table 1.

[0070] Comparative Example 4

[0071] According to the preparation method disclosed in CN106513006A, β molecular sieve was added to the powder and mixed evenly to prepare a reference agent H having the same catalyst composition as Example 1 of the present invention. The specific process is as follows:

[0072] The basic nickel carbonate and 300 ml of deionized water were uniformly mixed and added to a 1L high-pressure ultrasonic reactor. The ultrasonic frequency was set to 60 KHz, and the mixture was heated to 80°C. After the temperature was kept constant for 1 hour, the ultrasonic frequency was reduced to 20 KHz, the system temperature was increased to 120°C, ammonium molybdate and polyvinyl pyrrolidone were added, and then 10 ml of 25wt% ammonia water was dropwise added to the system. After the temperature was kept constant for 2 hours, the ultrasound was turned off, the stirring was turned on, the speed was 300 rpm, ammonium metatungstate was added, and then citric acid was added until the pH of the system was 4.2. After the temperature was kept constant for 2 hours, the heating was turned off, and the slurry was collected after the system was cooled to room temperature. The slurry was spray-dried, and the inlet temperature and outlet temperature were controlled at about 200°C and 100°C, respectively. The obtained dry powder was roasted at 330°C in a muffle furnace for 3 hours to obtain an active component powder. β molecular sieve was added to the powder and mixed evenly. The active component powder, β molecular sieve mixture and aluminum hydroxide dry glue accounting for 40% of the weight of the active component powder were mixed, and then a 10% dilute nitric acid aqueous solution was added for kneading and extrusion to obtain strips with a diameter of 1.5 mm. The strips were dried at 110°C for 10 h and calcined in a muffle furnace at 400°C for 5 h to obtain reference agent H. The catalyst composition and main properties are shown in Table 1.

[0073] Comparative Example 5

[0074] The same as Example 1, the reference agent I was prepared, and all the sodium aluminate B solution and the β molecular sieve slurry were added at one time during the aging process of the precipitate slurry containing nickel, molybdenum, tungsten and aluminum, and the aging pH value was fixed. The specific preparation process is as follows:

[0075] Ammonium metatungstate and ammonium molybdate are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W and Mo. The weight concentration of W in the solution containing W and Mo is 68g / L in terms of WO3, and the weight concentration of Mo in terms of MoO3 is 32g / L. Nickel chloride is added to a dissolving tank 2 filled with deionized water to prepare a Ni-containing solution. The weight concentration of Ni in the Ni-containing solution is 52g / L in terms of NiO, and Al in the sodium metaaluminate B solution accounts for 30% of the total Al (in terms of Al2O3) in the obtained hydrocracking catalyst. Deionized water and isomeric tridecanol ether phosphate (E-1310P) with a molar ratio of 0.9 to the total number of Al atoms in the sodium metaaluminate solution A are added to a reaction tank, and CO2 gas with a concentration of 52v% is introduced into the reaction tank solution, and the flow rate of the CO2 gas is 80ml / min. The solution containing W and Mo and sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 is 8.4g / L) are added to the reaction tank in parallel to carry out gelling reaction. The reaction pH value is controlled at 5.4 and the reaction temperature is 62°C. After the reaction for 0.8 hours, the Ni-containing solution and sodium hydroxide solution (weight concentration is 10%) are added dropwise to the reaction slurry at the same time. The reaction temperature remains unchanged and the reaction time is 1.0 hour. The pH value is controlled at 8.8 at the end of the reaction. The introduction of CO2 gas is stopped at the end of the reaction to generate a precipitate slurry containing nickel, molybdenum, tungsten, aluminum and phosphorus. The resulting slurry is aged. At the beginning of aging, all sodium aluminate solution B and β molecular sieve slurry are added. The aging temperature is 78°C. The pH value is controlled to be 8.5 during aging. After aging for 4.0 hours, the aging is terminated. The resulting slurry is filtered and the filter cake is dried for the first time, dried at 100°C for 9 hours, rolled and extruded. Wash with deionized water at room temperature until neutral. Then the washed wet strips were dried as follows: first, the material was dried at 78°C for 7.5 hours, deionized water was evenly sprayed on the dried material, and then dried, and the uniform spraying of deionized water and drying process were repeated 5 times, the first spraying of deionized water and the dried material volume ratio was 2.0:1, the drying temperature was 190°C, and the drying time was 2.0 hours, the second spraying of deionized water and the dried material volume ratio was 1.5:1, the drying temperature was 190°C, and the drying time was 2.2 hours, the third spraying of deionized water and the dried material volume ratio was 1:1, the drying temperature was 180°C, and the drying time was 1.8 hours, the fourth spraying of deionized water and the dried material volume ratio was 1:1.8, the drying temperature was 180°C, and the drying time was 1.8 hours, and the fifth spraying of deionized water and the dried material volume ratio was 1:2.3, the drying temperature was 200°C, and the drying time was 1.9 hours. The dried material was calcined at 540°C for 4 hours to obtain catalyst I. The catalyst composition and main properties are shown in Table 1.

[0076] Comparative Example 6

[0077] The same method as in Example 1 was used to prepare the reference agent J. During the preparation process, the second drying of the molded product after washing adopted the first drying condition (conventional drying condition). The specific preparation process is as follows:

[0078] Ammonium metatungstate and ammonium molybdate are added to dissolving tank 1 filled with deionized water to prepare a solution containing W and Mo. The weight concentration of W in the solution containing W and Mo is 68 g / L as WO3, and the weight concentration of Mo in the solution containing MoO3 is 32 g / L. Nickel chloride is added to dissolving tank 2 filled with deionized water to prepare a Ni-containing solution. The weight concentration of Ni in the Ni-containing solution is 52 g / L as NiO. Aluminum chloride is added to dissolving tank 3 filled with deionized water. Al in sodium metaaluminate solution B accounts for 30% of the total Al (as Al2O3) in the obtained hydrocracking catalyst. It is divided into 5 equal parts by volume. The β molecular sieve slurry is prepared at a solid-liquid ratio of 1:3 and divided into 5 equal parts by volume. Deionized water and isomeric tridecanol ether phosphate (E-1310P) with a molar ratio of 0.9 to the total number of Al atoms in sodium aluminate solution A are added to the reaction tank, and CO2 gas with a concentration of 52v% is introduced into the reaction tank solution at a flow rate of 80ml / min. A solution containing W and Mo and a sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 is 8.4 g / L) are added to a reaction tank in parallel to carry out a gelling reaction. The reaction pH is controlled at 5.4 and the reaction temperature is 62°C. After the reaction for 0.8 hour, a Ni-containing solution and a sodium hydroxide solution (weight concentration is 10%) are simultaneously added dropwise to the reaction slurry. The reaction temperature remains unchanged and the reaction time is 1.0 hour. At the end of the reaction, the pH is controlled at 8.8. After the reaction is completed, the introduction of CO2 gas is stopped to generate a precipitate slurry containing nickel, molybdenum, tungsten, aluminum and phosphorus. The resulting slurry is aged at an aging temperature of 78°C. During aging, an equal portion of sodium aluminate solution B is first added to control the pH to 13.1, and an equal portion of β molecular sieve slurry is added. After an aging time of 0.3 hour, the aging pH is controlled at 9.6. After an aging time of 0.2 hour, the pH is then controlled to 7.5 for 0.3 hour. The above operation process is repeated 5 times to terminate the aging. The obtained slurry was filtered, and the filter cake was dried for the first time at 100°C for 9 hours, rolled, and extruded into strips. The wet strips were washed with deionized water at room temperature until neutral. The washed wet strips were dried at 100°C for 9 hours, and the dried material was calcined at 540°C for 4 hours to obtain catalyst J. The catalyst composition and main properties are shown in Table 1.

[0079] Comparative Example 7

[0080] The same method as in Example 1 was used to prepare reference agent L. During the preparation process, only deionized water was added to the reaction tank without adding castor oil phosphate. Meanwhile, carbon dioxide gas was not introduced during the reaction process. The specific reaction process is as follows:

[0081] Ammonium metatungstate and ammonium molybdate are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W and Mo. The weight concentration of W in the solution containing W and Mo is 68 g / L as WO3, and the weight concentration of Mo in the solution containing MoO3 is 32 g / L. Nickel chloride is added to a dissolving tank 2 filled with deionized water to prepare a Ni-containing solution. The weight concentration of Ni in the Ni-containing solution is 52 g / L as NiO. Al in the sodium metaaluminate solution B accounts for 30% of the total Al (as Al2O3) in the obtained hydrocracking catalyst, and it is divided into 5 equal parts by volume. The beta molecular sieve slurry is prepared at a solid-liquid ratio of 1:3 and divided into 5 equal parts by volume. Deionized water was added to the reaction tank, and the solution containing W and Mo and sodium aluminate solution A (the weight concentration of Al in terms of Al2O3 was 8.4 g / L) were added to the reaction tank in parallel for gelation reaction. The reaction pH was controlled at 5.4 and the reaction temperature was 62°C. After the reaction for 0.8 hour, the Ni-containing solution and sodium hydroxide solution (weight concentration was 10%) were simultaneously added dropwise to the reaction slurry. The reaction temperature remained unchanged and the reaction time was 1.0 hour. At the end of the reaction, the pH was controlled at 8.8 to generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum. The resulting slurry was aged at an aging temperature of 78°C. During aging, an equal portion of sodium aluminate solution B was first added to control the pH to 13.1, and an equal portion of β molecular sieve slurry was added. After the aging time of 0.3 hour, the aging pH was controlled at 9.6. After the aging time of 0.2 hour, the pH was then controlled to 7.5 for 0.3 hour. The above operation process was repeated 5 times to end the aging. The obtained slurry was filtered, and the filter cake was dried for the first time at 100°C for 9 hours, rolled, extruded and washed with deionized water at room temperature until neutral. Then the washed wet strips were dried as follows: first, the material was dried at 78°C for 7.5 hours, deionized water was evenly sprayed on the dried material, and then dried, and the uniform spraying of deionized water and drying process were repeated 5 times, the first spraying of deionized water and the dried material volume ratio was 2.0:1, the drying temperature was 190°C, and the drying time was 2.0 hours, the second spraying of deionized water and the dried material volume ratio was 1.5:1, the drying temperature was 190°C, and the drying time was 2.2 hours, the third spraying of deionized water and the dried material volume ratio was 1:1, the drying temperature was 180°C, and the drying time was 1.8 hours, the fourth spraying of deionized water and the dried material volume ratio was 1:1.8, the drying temperature was 180°C, and the drying time was 1.8 hours, and the fifth spraying of deionized water and the dried material volume ratio was 1:2.3, the drying temperature was 200°C, and the drying time was 1.9 hours. The dried material was calcined at 540°C for 4 hours to obtain catalyst K. The catalyst composition and main properties are shown in Table 1.

[0082] Example 5

[0083] This example is an activity evaluation experiment of the catalyst of the present invention, and is compared with the comparative catalyst. The comparative evaluation test was carried out on a 200mL small hydrogenation device using the catalysts A, B, C, D of the present invention and the comparative catalysts E, F, G, H, I, J, and K, respectively. The evaluation conditions are: total reaction pressure 15.7MPa, hydrogen-to-oil volume ratio 1200:1, liquid hourly volume space velocity 1.6h- 1 , reaction temperature 375 ℃, 385 ℃, the raw material for evaluation is vacuum wax oil, its main properties are shown in Table 4, and the evaluation results are shown in Tables 5-6. It can be seen from Tables 1-3 that the average particle size of the catalyst oxide particles of the present invention is small and evenly distributed, the surface active metal is more, the surface pore size is larger, and there is good synergy between the acidic component and the hydrogenation component. Catalyst activity evaluation process conditions and evaluation results show that compared with the comparative catalyst, the active metal distribution, pore size distribution and average particle size of the oxide particles of the catalyst of the present invention are smaller and evenly distributed, which are beneficial to improving the aromatic saturation performance. The catalyst of the present invention has both high isomerization performance and high aromatic saturation performance in the process of treating heavy raw material oil hydrocracking. The properties such as the pour point and aromatic content of the diesel fraction can meet the standards of industrial-grade white oil and transformer oil, and can flexibly produce special oils such as transformer oil, white oil and high viscosity index lubricating oil base oil raw materials. The comparative catalyst cannot have high isomerization performance and high aromatic saturation performance at the same time. The hydrocracking catalyst of the present invention still has good stability and good product quality under high nitrogen content feed conditions.

[0084] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples

[0085]

[0086]

[0087] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples

[0088]

[0089] Table 2 Ratio of the weight content of active metal oxides on the catalyst surface to the weight content of active metal oxides in the bulk phase

[0090] Catalyst No. A B C D E F <![CDATA[Surface I W+Ni / Bulk I W+Ni > 5.38 5.19 5.60 5.82 0.92 1.02 <![CDATA[Surface I Mo + Ni / Bulk I Mo + Ni > 4.38 4.28 4.57 4.69 1.03 0.99

[0091] Table 2

[0092] Catalyst No. G H I J K <![CDATA[Surface I W+Ni / Bulk I W+Ni > 4.41 1.18 3.98 5.02 4.64 <![CDATA[Apparent Phase I Mo + Ni / Bulk Phase I Mo + Ni > 3.68 0.90 2.78 4.12 3.81

[0093] Table 3 Average particle size and particle size distribution of the catalyst oxide particles obtained in each example

[0094] Catalyst No. A B C D E F Average particle size of oxide particles, nm 11.9 12.2 11.6 11.2 26.5 28.9 Oxide particle size distribution, % Particle size less than 10nm 8.89 8.28 9.05 9.21 2.36 2.03 Particle size is 10nm-14nm 80.64 79.91 81.07 81.67 10.98 8.56 Particle size greater than 14nm 10.47 11.81 9.88 9.12 86.66 89.41

[0095] Table 3 Average particle size and particle size distribution of the catalyst oxide particles obtained in each example

[0096] Catalyst No. G H I J K Average particle size of oxide particles, nm 12.0 22.3 18.5 12.3 25.3 Oxide particle size distribution, % Particle size less than 10nm 8.82 3.18 6.86 8.78 3.12 Particle size is 10nm-14nm 80.55 11.61 47.89 79.54 34.69 Particle size greater than 14nm 10.63 85.21 45.25 11.68 61.19

[0097] Table 4 Main properties of crude oil

[0098]

[0099]

[0100] Table 5 Evaluation results of catalysts of Examples and Comparative Examples (operation for 250 hours)

[0101] catalyst A B C D E F Reaction temperature, °C 375 375 375 375 375 375 Nitrogen content in feed, μg / g 118 102 135 109 118 118 82~132℃ heavy naphtha Aromatic potential, wt% 58.4 58.7 58.0 58.1 61.0 61.2 132~282℃ Aviation fuel Smoke point / mm 29.6 29.4 29.8 29.9 23.4 24.1 Aromatics, v% 1.6 1.7 1.4 1.2 10.2 9.8 282~370℃ diesel Pour point / ℃ -7 -7 -7 -8 -7 -7 Aromatics / wt% 2.3 2.6 2.1 2.0 13.5 12.7 >370℃ tail oil BMCI value 5.8 6.0 5.5 5.2 23.9 23.3 Viscosity Index 123 122 125 127 88 91

[0102] Table 5 Evaluation results of catalysts of Examples and Comparative Examples (running for 250 hours)

[0103]

[0104]

[0105] Table 6 Evaluation results of catalysts of Examples and Comparative Examples (operation 2000 hours)

[0106] catalyst A B E F I J Reaction temperature, °C 375 375 385 385 385 385 Nitrogen content in feed, μg / g 118 102 118 118 118 118 82~132℃ heavy naphtha Aromatic potential, wt% 58.6 58.9 62.2 62.4 62.0 62.6 132~282℃ Aviation fuel Smoke point / mm 29.5 29.3 21.8 21.4 22.6 21.0 Aromatics, v% 1.8 2.0 19.1 19.9 18.0 20.9 282~370℃ diesel Pour point / ℃ -7 -7 -7 -8 -8 -9 Aromatics / wt% 2.5 2.8 18.0 19.2 17.6 20.6 >370℃ tail oil BMCI value 5.9 6.1 31.5 32.9 30.4 34.6 Viscosity Index 122 121 80 79 82 77

[0107] Table 7 Properties of β molecular sieves in Examples and Comparative Examples

[0108] Silicon to aluminum molar ratio 80.5 <![CDATA[Specific surface area, m 2 / g]]> 621 Pore ​​volume, mL / g 0.55 IR total acid, mmol / g 0.43 <![CDATA[Na2O,wt%]]> 0.080

[0109] Table 8 Properties of Y-type molecular sieve used in the present invention

[0110] Molecular sieve properties Y Relative crystallinity, % 110 Unit cell parameters, nm 2.431 <![CDATA[Molar ratio of SiO2 / Al2O3]]> 80.8 <![CDATA[Specific surface area, m 2 / g]]> 896 Pore ​​volume, mL / g 0.510 IR total acid, mmol / g 0.248 B acid / L acid 11.64 <![CDATA[Na2O,wt%]]> <0.01

Claims

1. A method for preparing a bulk hydrocracking catalyst, characterized in that The method comprises the following contents: (1) adding deionized water and phosphate to a reaction tank, continuously introducing CO2, and adding a solution containing W and Mo and a sodium aluminate solution A to the reaction tank in parallel for gelation reaction to obtain material A; (2) adding a solution containing Ni and a precipitant aqueous solution to the material A obtained in step (1), reacting the material A, and then subjecting the material to aging treatment. During the aging process, sodium aluminate solution B and β molecular sieve slurry are added n times to obtain a slurry which is filtered to obtain material B; wherein the sodium aluminate solution B and β molecular sieve slurry are added n times in the manner of first adding 1 / n volume of sodium aluminate solution B and then adding 1 / n volume of β molecular sieve slurry each time, and the process is performed n times in total, where n is an integer between 2 and 8; (3) The material B obtained in step (2) is first dried, rolled, formed, washed, and then second dried and calcined to obtain a bulk hydrocracking catalyst.

2. The method according to claim 1, characterized in that: The phosphate ester in step (1) is one or more of octadecyl ether phosphate, alkylphenol ether phosphate, isomeric tridecyl alcohol ether phosphate, lauryl alcohol ether phosphate, castor oil phosphate, octadecyl phosphate, and lauryl phosphate; the molar ratio of the phosphate ester to Al in the sodium aluminate solution in step (1) is 0.2:1 to 2.0:

1.

3. The method according to claim 1, characterized in that: The concentration of the added CO2 gas in step (1) is 40v% to 70v%; the flow rate of the CO2 gas is 30 to 120mL / min. After the gelling reaction is completed, the introduction of the CO2 gas is stopped.

4. The method according to claim 1, characterized in that: In the W- and Mo-containing solution of step (1), the weight concentration of W calculated as WO3 is 5 to 120 g / L, and the weight concentration of Mo calculated as MoO3 is 5 to 110 g / L; the concentration of the sodium aluminate solution A is 5 to 90 g / L in terms of Al2O3 concentration.

5. The method according to claim 1, characterized in that: The conditions of the gelling reaction in step (1) are as follows: the reaction temperature is 30 to 95° C., preferably 40 to 95° C., the pH value of the co-current reaction is controlled at 5 to 6, and the reaction time is 0.1 to 1.0 hour.

6. The method according to claim 1, characterized in that: In the Ni-containing solution of step (2), the weight concentration of Ni calculated as NiO is 5 to 130 g / L, preferably 10 to 115 g / L; in the sodium aluminate solution B, the weight concentration of Al calculated as Al2O3 is 5 to 70 g / L, preferably 8 to 60 g / L.

7. The method according to claim 1, characterized in that: In step (2), the sodium aluminate solution B is divided into n equal parts by volume, wherein n is an integer of 2 to 8; and the β molecular sieve slurry is divided into n equal parts by volume, wherein n is an integer of 2 to 8.

8. The method according to claim 1, characterized in that: The precipitating agents described in step (2) are all alkaline precipitating agents, selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium hydroxide, potassium carbonate or potassium bicarbonate.

9. The method according to claim 1, characterized in that: The reaction conditions of step (2) are as follows: the reaction temperature is 30-95° C., the pH value is controlled at 8.0-12.0 at the end, and the reaction time is 0.5-2.5 hours.

10. The method according to claim 1, characterized in that: The aging treatment conditions in step (2) are as follows: the aging temperature is 60-98° C.; the aging process is carried out in the following manner: n times of three-stage decreasing pH aging are performed, and in each three-stage decreasing pH aging, when adjusting the pH value in the first stage, 1 / n volume of sodium aluminate solution B is used for adjustment, and after adjustment, 1 / n volume of β molecular sieve slurry is added; The three-level decreasing pH aging is as follows: the first level, the pH value is 11.0-13.5, the aging time is 0.05-0.5 hours, the second level, the pH value is adjusted to 8.5-10.5, the aging time is 0.05-0.5 hours, the third level, the pH value is adjusted to 4.5-6.2, the aging time is 0.05-0.5 hours.

11. The method according to claim 1, characterized in that: In step (2), the Al added to the sodium aluminate solution B accounts for 5% to 55% of the total Al in the obtained catalyst calculated as Al2O3.

12. The method according to claim 1, characterized in that: The beta molecular sieve described in step (2) has the following properties: a molar ratio of silicon oxide to aluminum oxide of 30 to 90; a specific surface area of ​​430 to 780 m 2 / g, pore volume is 0.30~0.90cm 3 / g, the infrared acid content is 0.10~0.45mmol / g; the beta molecular sieve slurry is a uniform mixture of beta molecular sieve and deionized water, and the solid-liquid mass ratio is 1:1.1~1:5.

5.

13. The method according to claim 1, characterized in that: The first drying, molding and washing described in step (3) are carried out by conventional methods in the art; the first drying conditions are as follows: drying at 40-150°C for 1-48 hours; one or more of a peptizing agent and an extrusion aid are added as needed during the molding process; the peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, and oxalic acid; the extrusion aid is one or more of sesbania powder, carbon black, graphite powder, and citric acid, and the amount of the extrusion aid accounts for 1wt% to 10wt% of the total material dry basis. Washing is carried out with deionized water or a solution containing a decomposable salt until it is neutral.

14. The method according to claim 1, characterized in that: The second drying process described in step (3) is as follows: a. First, dry the material at 60-100°C for 1.0-8.5 hours; b. Evenly spray water on the material obtained in step a, with the volume ratio of water to dry material being 1:4-4:1, and then dry at a temperature of 150-280°C for 0.5-4.0 hours; c. Repeat step b 2-9 times; wherein the volume ratio of the first water addition volume to the dry material is greater than 1:1, and the volume ratio of the last water addition volume to the dry material is less than 1:1, and further, the volume ratio of the water addition volume to the dry material gradually decreases with the increase in the number of repetitions; further, the total drying time used for the second drying is preferably 5-40 hours.

15. The method according to claim 1, characterized in that: The calcination conditions of step (3) are as follows: calcination at 350-650° C. for 1-24 hours, preferably calcination at 400-600° C. for 2-12 hours.

16. A hydrocracking catalyst, characterized in that: The catalyst is a bulk hydrocracking catalyst, which comprises a hydrogenation active metal component, amorphous alumina and a beta molecular sieve; the catalyst particles comprise an outer surface layer, an intermediate layer and a central core, and the average pore diameter decreases in a gradient, that is, the average pore diameter of the outer surface layer is greater than the average pore diameter of the intermediate layer, and the average pore diameter of the intermediate layer is greater than the average pore diameter of the central core; the average pore diameter of the outer surface layer is 11-19 nm, the average pore diameter of the intermediate layer is 7-11 nm, and the average pore diameter of the central core is 3-7 nm, wherein on the cross section of the catalyst particle, the length from the outermost edge to the center point is R; the thickness of the outer surface layer is 0.2R-0.4R, the thickness of the intermediate layer is 0.2R- 0.5R, and the rest is the central core; the molar ratio of W / Mo is 1:5~21:1, preferably 1:3~19:1, and the molar ratio of Ni / (Mo+W) is 1:14~16:1, preferably 1:12~14:1; wherein the ratio of the sum of the weight contents of the surface active metal components WO3 and NiO to the sum of the weight contents of the bulk active metal components WO3 and NiO is 2.8:1~6.5:1, preferably 3.4:1~6.2:1, and the ratio of the sum of the weight contents of the surface active metal components MoO3 and NiO to the sum of the weight contents of the bulk active metal components MoO3 and NiO is 2.0:1~5.5:1, preferably 2.2:1~5.2:

1.

17. The catalyst according to claim 16, characterized in that: The average particle size of tungsten, molybdenum and nickel active metal oxide particles is 10~14nm; the particle size distribution of the oxide particles is as follows: the number of particles with a particle size less than 10nm accounts for 2%~17% of the total number of particles, the number of particles with a particle size of 10nm~14nm accounts for 72%~90% of the total number of particles, and the number of particles with a particle size greater than 14nm accounts for 3%~19% of the total number of particles.

18. Use of the catalyst according to claim 16 in a hydrocracking process for producing base oil for special oil and lubricating oil.

Citation Information

Patent Citations

  • Hydrated alumina composition containing BETA molecular sieve, molding body, preparation methods of hydrated alumina composition containing BETA molecular sieve, and molding body, applications of molding body, and catalyst and preparation method thereof

    CN107999120A

  • Production method of hydrocracking catalyst

    CN110038621A

  • Preparation method of bulk phase hydrocracking catalyst

    CN114471687A