Preparation method of bulk phase hydrocracking catalyst

By controlling the incremental pH value and multiple aging during the preparation process of the hydrocracking catalyst, and adding β molecular sieve slurry, the problem of insufficient isomerization performance and aromatic conversion ability of the existing catalyst is solved, and the nitrogen tolerance of the catalyst is improved. performance and product quality, suitable for the production of industrial grade white oils and lubricants.

CN118767976AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310369740.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Existing hydrocracking catalysts are difficult to balance between high isomerization performance and high aromatics conversion capacity, and their nitrogen resistance is insufficient to meet the production requirements of industrial white oil and lubricating base oils.

Method used

By co-currently carrying out a gel-forming reaction with a solution containing W, Ni, and Al and a precipitant, controlling the pH value to increase gradually and adding the molybdenum-containing solution, and then performing multiple aging and adding β molecular sieve slurry, and finally drying and roasting, a polymer with a Catalysts with uniformly dispersed active metals and small and uniform oxide particle sizes enhance the pore volume and pore size distribution of the catalyst and promote the synergistic effect of acidic and hydrogenation components.

Benefits of technology

The prepared catalyst has excellent isomerization performance and aromatic hydrocarbon conversion ability, is suitable for the hydrocracking process of No. 5 industrial grade white oil and lubricating oil base oil, and improves the nitrogen resistance performance and product quality of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004168157570000151
    Figure BDA0004168157570000151
  • Figure BDA0004168157570000161
    Figure BDA0004168157570000161
  • Figure BDA0004168157570000162
    Figure BDA0004168157570000162
Patent Text Reader

Abstract

The invention discloses a preparation method of a bulk phase hydrocracking catalyst, which comprises the following steps: (1) adding a solution containing W, Ni and Al into a gelling reaction tank, and dropwise adding an alkaline precipitator for gelling reaction; the pH value is controlled to gradually increase from the initial value to the final value through an alkaline precipitator in the gelling reaction process, and a molybdenum-containing solution is added after each increasing; (2) continuously aging the slurry obtained in the step (1) for n times, adding 1 / n sodium metaaluminate solution and 1 / n beta molecular sieve slurry in each aging process, uniformly mixing, and filtering to obtain a solid-phase material; and (3) preparing the hydrocracking catalyst from the solid-phase material. The catalyst prepared by the method is uniform in active metal dispersion, large in surface phase active site density, small in oxide particle size and uniform in oxide particle distribution, good in nitrogen resistance and suitable for being applied to a hydrocracking process of No. 5 industrial grade white oil and lubricant base oil, and the active component and the acidic component have a good synergistic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum refining, and in particular relates to a method for preparing a bulk hydrocracking catalyst. Background Art

[0002] The hydrocracking diesel fraction has the characteristics of water white color, low impurity content, and high saturated hydrocarbon content. It can be blended to produce various white oils, anti-rust oils, transformer oils, aluminum cold rolling oils, etc. The hydrocracking tail oil fraction is suitable for lubricating oil base oil. Depending on the brand, the pour point index of industrial white oil is between -3 and -9°C, and the mass content of aromatics is required to be no more than 5%. Depending on the lowest cold operating temperature in actual application, the pour point index range of transformer oil is between -10°C and -50°C, and the content of polycyclic aromatic hydrocarbons is required to be less than 3%. According to the product indicators of special oils, the hydrocracking catalyst needs to have high isomerization performance and high aromatic conversion capacity. It is difficult for the existing hydrocracking catalyst system to take both into account. At present, the acidic components commonly used in hydrocracking are Y molecular sieve, β molecular sieve, and ZSM-5 molecular sieve. Among them, β molecular sieve has the best isomerization performance and can meet the pour point index requirements of industrial white oil. However, it is difficult for conventional supported hydrogenation catalysts and bulk catalysts prepared by existing technologies to meet the requirements for the content of polycyclic aromatic hydrocarbons in industrial white oil.

[0003] Hydrocracking is carried out under high pressure, and hydrocarbon molecules and hydrogen react on the catalyst surface to crack and hydrogenate to generate lighter molecules. Hydrodesulfurization, denitrogenation and hydrogenation of unsaturated hydrocarbons also occur. Traditional supported hydrocracking catalysts are limited by the pore structure of the carrier, and the active metal loading is generally not more than 30wt%. The hydrogenation activity of the catalyst is far from reaching the aromatic conversion activity when producing high value-added special oil products. The bulk hydrocracking catalyst prepared by coprecipitation has a high active metal content, but the oxide particles generated during the coprecipitation reaction are of different sizes, the pore volume and specific surface area of ​​the catalyst are small, and the active metal utilization rate is low. The molecular sieve is mostly added after the active metal precipitation is generated, and the pores of the oxide particles formed before and the molecular sieve pores cannot be interconnected, which reduces the mutual coordination between the acidic component and the hydrogenation component and the diffusion performance of the catalyst, thereby weakening the hydrocracking activity of the bulk catalyst. Therefore, the bulk catalyst produced by the existing technology still cannot meet the hydrogenation activity requirements required for the production of high value-added special oil products. At the same time, nitrogen compounds in hydrocracking feedstocks have different degrees of poisoning (shielding) effects on the acidic centers of hydrocracking catalysts, which requires improving the nitrogen resistance of hydrocracking catalysts. Hydrocracking catalysts have good nitrogen resistance, which can improve the raw material adaptability of the catalyst and extend the operating cycle of industrial equipment.

[0004] Bulk catalysts are currently the most active hydrogenation catalysts. Bulk hydrogenation catalysts can get rid of the limitation of metal content and can arbitrarily adjust the ratio of each active component in the catalyst to improve the hydrogenation performance of the catalyst. The combination of active metal components in the hydrogenation catalyst is more active than the individual components. Among the combinations of metal components, the W-Ni combination has the best hydrogenation saturation activity, and the Mo-Ni combination has the best hydrogenation denitrification. The size and distribution of metal oxide particles in bulk catalysts have a great influence on the distribution of hydrogenation active metals and the interaction between different hydrogenation active metals, which further affects the hydrogenation activity of bulk catalysts. At the same time, the catalyst pore size and specific surface area also affect the hydrogenation activity of bulk catalysts.

[0005] CN106179462A discloses a hydrocracking catalyst and a preparation method thereof, wherein the method first adopts a positive addition method to prepare a precipitate slurry I containing Ni and Al components, and then adopts a parallel flow method to prepare a precipitate slurry II containing W, Si and Al components, and the two precipitate slurries are mixed evenly, aged and filtered, and the obtained material is mixed with urea, subjected to hydrothermal treatment in water vapor, and then a Y-type molecular sieve suspension is added. The catalyst oxide obtained by the method is of different sizes, and the surface active metals are excessively accumulated after the hydrothermal treatment, and the utilization rate of the surface active metals is not improved. At the same time, after the molecular sieve is added, the interaction between the catalyst acid component and the hydrogenation component is greatly reduced.

[0006] CN103055923A discloses a method for preparing a hydrocracking catalyst. The method is as follows: preparing an acidic mixed solution A containing hydrogenation active metals and silicon, preparing an alkaline solution B of sodium metaaluminate, and then mixing the acidic mixed solution A, the alkaline solution B and gaseous CO 2 Add the mixture into a reaction tank filled with clean water to form a gel, add the suspension of Y-type molecular sieve and mix evenly, filter, dry, shape, wash, dry and roast to obtain a hydrocracking catalyst. This method can increase the pore volume and specific surface area of ​​the catalyst, but this method only relies on the carbonate generated in the precipitation to release gas during roasting to increase the pore volume, specific surface area and improve the dispersion of active catalyst metals. At the same time, it is easy to cause the active metals in the catalyst to aggregate.

[0007] CN110038617A discloses a hydrocracking catalyst and its preparation method. The hydrocracking catalyst is a bulk catalyst, which is prepared by firstly subjecting a mixed solution A containing Ni, W and Al components to a precipitant in parallel to a gelling reaction, subjecting the obtained slurry to preliminary aging, then subjecting a mixed solution B containing W, Si and Al components to a precipitant in parallel to the aged slurry to a reaction, then subjecting the precipitant to the addition of a molecular sieve suspension to aging, and then subjecting the catalyst to post-treatment to prepare a hydrocracking catalyst. The catalyst has a small specific surface area and pore volume, and its hydrogenation activity cannot meet the standards of industrial-grade white oil products.

[0008] The hydrogenation activity of catalysts prepared by existing technologies cannot meet the production of industrial white oil. Therefore, improving the hydrogenation activity of bulk catalysts and improving the coordination between hydrogenation components and acidic components are the key to ensuring that bulk hydrocracking catalysts meet the production of industrial white oil. Summary of the invention

[0009] In view of the deficiencies of the prior art, the present invention provides a method for preparing a bulk hydrocracking catalyst. The catalyst prepared by the method has uniform dispersion of active metals, large surface active site density, small oxide particle size and uniform distribution, good synergistic effect between active components and acidic components, and good nitrogen resistance. The catalyst prepared by the present invention has excellent isomerization performance and aromatic conversion ability, and is suitable for use in the hydrocracking process of No. 5 industrial grade white oil and lubricating oil base oil.

[0010] The method for preparing the bulk hydrocracking catalyst of the present invention comprises:

[0011] (1) adding a solution containing W, Ni and Al into a gelling reaction tank, and dripping a precipitant A and a precipitant B into the reaction tank in parallel to perform a gelling reaction; during the gelling reaction, the pH value is controlled by the precipitant to increase from an initial value to a final value, and a molybdenum-containing solution is added after each increase; the number of increases is 2 to 10 times, preferably 2 to 8 times;

[0012] (2) The slurry obtained in step (1) is aged for n times continuously, and 1 / n sodium aluminate solution and 1 / n beta molecular sieve slurry are added and mixed uniformly during each aging process, and the slurry obtained after aging is filtered to obtain a solid phase material; wherein the aging process adopts a stepwise decreasing pH value aging process;

[0013] (3) The solid phase material obtained in step (2) is dried, formed, washed, dried and calcined to obtain a hydrocracking catalyst.

[0014] In the method of the present invention, in the solution containing W, Ni and Al in step (1), W is in the form of WO 3 The weight concentration of Ni as NiO is 5 to 130 g / L, preferably 10 to 125 g / L, and the weight concentration of Al as Al is 5 to 140 g / L, preferably 15 to 130 g / L. 2 O 3 The weight concentration is 2 to 90 g / L, preferably 6 to 85 g / L; wherein, when preparing a solution containing W, Ni, and Al, the tungsten source generally used is ammonium metatungstate, the aluminum source is one or more of aluminum nitrate, aluminum sulfate, aluminum chloride, and aluminum acetate, and the nickel source is generally one or more of nickel sulfate, nickel nitrate, and nickel chloride.

[0015] In the method of the present invention, the precipitant A described in step (1) is a mixed solution of sodium hydroxide and sodium bicarbonate, the precipitant B is ammonia water, the concentration of the mixed solution of sodium hydroxide and sodium bicarbonate is 7wt%-20wt%, the molar ratio of sodium hydroxide to sodium bicarbonate is 0.2:1-0.8:1, preferably 0.3:1-0.7:1, the concentration of ammonia water is 4wt%-8wt%, and the molar ratio of ammonia water to the mixed solution of sodium hydroxide and sodium bicarbonate is 0.1:1-0.45:1, preferably 0.15:1-040:1.

[0016] In the method of the present invention, when the gelling reaction described in step (1) starts, a precipitant is used to control the initial pH value to 5.0-6.5; the final pH value is 8.0-10.5, the gelling reaction temperature is 40-90° C., and the gelling reaction time is 0.3-6.0 hours.

[0017] In the method of the present invention, during the gelling reaction described in step (1), the pH value is preferably kept constant for 0.05 to 0.5 hours after each increase. The increment of each pH value may be the same or different. Preferably, the increment of the pH value is not greater than the increment of the previous pH value.

[0018] In the method of the present invention, in the Mo-containing solution of step (1), Mo is in the form of MoO 3 The weight concentration is 10-150 g / L, preferably 10-140 g / L; when preparing a solution containing Mo, the molybdenum source is generally ammonium molybdate. The molybdenum-containing solution is added in batches according to the increasing number of pH values, and the volume of the molybdenum-containing solution added each time can be the same or different, and the total amount of the molybdenum-containing solution is determined according to the catalyst composition.

[0019] In the method of the present invention, the sodium aluminate solution in step (2) is Al 2 O 3 The weight concentration is 5-75 g / L, preferably 8-65 g / L. The sodium aluminate solution is divided into n parts (n is 2-8) by volume according to the number of additions, preferably divided equally by volume. The β molecular sieve slurry is divided into n parts (n is 2-8) by volume according to the number of additions, preferably divided equally by volume.

[0020] In the method of the present invention, the aging temperature in step (2) is 60 to 98°C, preferably 65 to 92°C.

[0021] In the method of the present invention, the pH value of step (2) is gradually reduced in the aging process: the reaction slurry is dripped into a 1 / n sodium aluminate solution to adjust the pH value, the pH value is controlled at 11.5-13.5, 1 / n β molecular sieve slurry is added, and the aging is performed for 0.05-0.5 hours; then the pH value is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; finally, the pH value is adjusted to 4.0-6.5, and the aging time is 0.05-0.5 hours, wherein n is an integer of 2-8. And so on (i.e., the pH value is re-controlled to 11.0-13.5, and the aging time is 0.05-0.5 hours).

[0022] Among them, except for the use of sodium aluminate solution in the first stage pH value adjustment during the aging process, the acids and alkalis used for adjusting the pH value can be inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements. The inorganic acid can be hydrochloric acid and acetic acid, and the inorganic alkali can be one or more of sodium carbonate, sodium bicarbonate, ammonia water, and sodium hydroxide. The concentration and dosage of the acid and alkali solutions can be adjusted according to the actual preparation needs.

[0023] In the method of the present invention, in step (2), the Al added to the sodium aluminate solution accounts for 1:1 of the total Al in the obtained hydrocracking catalyst. 2 O 3 5% to 50%, preferably 6% to 45%.

[0024] In the method of the present invention, the beta molecular sieve described in step (2) has the following properties: a molar ratio of silicon oxide to aluminum oxide of 30 to 90; a specific surface area of ​​430 to 780 m 2 / g, preferably 400-700m 2 / g; pore volume is 0.30~0.90cm 3 / g, preferably 0.35 to 0.85 cm 3 / g; the infrared acid content is 0.10-0.45mmol / g, preferably 0.18-0.40mmol / g. The β molecular sieve slurry is a mixture of β molecular sieve and deionized water after being stirred evenly, and the solid-liquid mass ratio is 1:1.2-1:5.5.

[0025] In the method of the present invention, the drying, molding and washing described in step (3) can be carried out by conventional methods in the art. The drying conditions are as follows: drying at 40-150°C for 1-48 hours, preferably drying at 50-120°C for 4-36 hours. During the molding process, conventional molding aids, such as one or more of peptizers, extrusion aids, etc., can be added as needed. The peptizer is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the extrusion aid refers to a substance that is conducive to extrusion molding, such as one or more of sesbania powder, carbon black, graphite powder, citric acid, etc., and the amount of the extrusion aid accounts for 1wt% to 10wt% of the total material dry basis. Washing is generally carried out with deionized water or a solution containing decomposable salts (such as ammonium acetate, ammonium chloride, ammonium nitrate, etc.) until neutral. In the preparation method of the hydrocracking catalyst of the present invention, the shape of the catalyst can be flake, spherical, cylindrical and shaped (three-leaf clover, four-leaf clover) as required, preferably cylindrical and shaped (three-leaf clover, four-leaf clover). The diameter of the catalyst can be a thin strip of 0.8-2.0 mm or a thick strip of >2.5 mm.

[0026] In the method of the present invention, the calcination conditions in step (3) are as follows: calcination at 350-650° C. for 1-24 hours, preferably calcination at 400-600° C. for 2-12 hours.

[0027] The present invention also provides a bulk hydrocracking catalyst, which includes a hydrogenation active metal component, amorphous alumina and beta molecular sieve; the pore size distribution of the hydrocracking catalyst is as follows: the pore volume occupied by pores with a diameter of less than 6nm accounts for 2% to 14% of the total pore volume, the pore volume occupied by pores with a diameter of 6 to 10nm accounts for 55% to 75% of the total pore volume, the pore volume occupied by pores with a diameter of 10 to 15nm accounts for 9% to 25% of the total pore volume, and the pore volume occupied by pores with a diameter of more than 15nm accounts for 8% to 23% of the total pore volume. The specific surface area of ​​the catalyst is 200 to 600m 2 / g, pore volume is 0.28~1.2mL / g. The molar ratio of W / Mo is 1:13~10:1, preferably 1:11~9:1, and the molar ratio of Ni / (Mo+W) is 1:14~13:1, preferably 1:12~12:1; wherein the surface active metal component WO 3 The sum of the weight contents of NiO and bulk active metal components WO 3 The weight ratio of the total weight of MoO to NiO is 2.4:1 to 6.5:1, preferably 3.5:1 to 6.2:1, and the surface active metal component MoO 3 The sum of the weight contents of NiO and bulk active metal components MoO 3 The ratio of the sum of the weight contents of NiO to that of NiO is 2.3:1 to 5.6:1, preferably 2.5:1 to 5.3:1.

[0028] In the catalyst of the present invention, the average particle size of the active metal oxide particles of tungsten, molybdenum and nickel is 8 to 12 nm. Preferably, the particle size distribution of the oxide particles is as follows: the number of particles with a particle size less than 8 nm accounts for 3% to 15% of the total number of particles, the number of particles with a particle size of 8 nm to 12 nm accounts for 70% to 90% of the total number of particles, and the number of particles with a particle size greater than 12 nm accounts for 6% to 18% of the total number of particles.

[0029] In the preparation method of the hydrocracking catalyst of the present invention, the shape of the catalyst can be flake, spherical, cylindrical and shaped (three-leaf clover, four-leaf clover) as required, preferably cylindrical and shaped (three-leaf clover, four-leaf clover). The diameter of the catalyst can be a thin strip of 0.8-2.0 mm or a thick strip of >2.5 mm.

[0030] The hydrocracking catalyst of the present invention can be used in the hydrocracking process of base oil for producing special oil and lubricating oil, and is particularly suitable for the hydrocracking process of base oil raw materials of No. 5 industrial grade white oil and high viscosity index lubricating oil.

[0031] The hydrocracking catalyst of the present invention is applicable to a wide range of heavy raw materials, including one or more of various hydrocarbon oils such as vacuum gas oil, coking gas oil, deasphalted oil, thermal cracking gas oil, catalytic cracking gas oil, catalytic cracking circulating oil, etc., usually containing hydrocarbons with a boiling point of 250-550°C, and a nitrogen content of 300-2500 μg / g. After the hydrocracking pretreatment process, the nitrogen content in the feed of the hydrocracking catalyst of the present invention is less than 150 μg / g, that is, the nitrogen content in the feed of the hydrocracking catalyst reaction section is less than 150 μg / g, further more than 10 μg / g, even more than 50 μg / g. The hydrocracking catalyst of the present invention still has high activity, stability and good product quality under high nitrogen content feed conditions (less than 150 μg / g).

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] 1. The method of the present invention controls the preparation steps and preparation conditions comprehensively, so that the oxide particles have a small particle size and are evenly distributed, and can fully contact with the molecular sieve. At the same time, the pore volume and pore size of the catalyst are increased, and the pore size distribution is concentrated in 6-10nm, which increases the probability of the active component carrier pores and the molecular sieve pores to interpenetrate each other, improves the diffusion performance of the catalyst and the coordination between the hydrogenation component and the acidic component. The enhanced hydrogenation activity of the catalyst can hydrogenate more and faster organic nitrogen-containing compounds that have a large poisoning effect on the acidic center of the catalyst, plays a protective role on the acidic center of the catalyst, improves the nitrogen resistance of the hydrocracking catalyst, and can also improve the properties of the hydrocracking product.

[0034] 2. The present invention adopts a mixed solution of sodium hydroxide and sodium carbonate and ammonia water as precipitants during the reaction process. By controlling the mass ratio of sodium hydroxide and sodium carbonate and the weight concentration of ammonia water, compared with single precipitants such as ammonia water, sodium hydroxide and sodium carbonate, the present invention effectively overcomes the problems of small pore volume and specific surface area of ​​bulk catalysts, poor adhesion of gelling materials, large oxide particles, etc., and the generated particles are uniform in size, which is more conducive to the interaction between acid centers and hydrogenation centers.

[0035] 3. The present invention precipitates a solution containing W, Ni and Al at a specific pH value by using a step-by-step pH value gelling method, thereby preventing the generation of large oxide particles during the gelling process and dispersing the active metals evenly. The addition of Mo during the step-by-step pH value increase process is more conducive to the interaction between the active metals, thereby greatly improving the hydrogenation activity of the catalyst.

[0036] 4. In the present invention, the pH value is swung during aging and sodium aluminate solution is added in batches. The pH value swing is used to dissolve the amorphous oxide in the oxide particles. The addition of sodium aluminate solution re-modifies the size of the oxide particles. With each simultaneous addition of molecular sieves, the metal oxide particles are in better contact with the molecular sieves, thereby promoting a synergistic effect. DETAILED DESCRIPTION

[0037] In the present invention, the specific surface area and pore volume are measured by low-temperature liquid nitrogen adsorption method, and the mechanical strength is measured by lateral pressure method.

[0038] In the present invention, the active metal content of the catalyst surface phase is measured by X-ray photoelectron spectroscopy (XPS), and the active metal content of the catalyst bulk phase is measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES).

[0039] In the present invention, wt% refers to mass fraction, and v% refers to volume fraction.

[0040] In the present invention, the average particle size (D50 particle size) and particle size distribution of the active metal oxide particles are measured using a nanoparticle size and Zeta potential analyzer (Zetasizer Nano ZS).

[0041] In the present invention, the properties of the β molecular sieve used are shown in Table 7, and the properties of the Y molecular sieve are shown in Table 8.

[0042] Example 1

[0043] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. In the solution containing W, Ni and Al, W is WO 3 The weight concentration of Ni as NiO is 58g / L, the weight concentration of Al as Al is 44g / L. 2 O3 The weight concentration is 28 g / L. Ammonium molybdate is added to the dissolution tank 2 filled with deionized water to prepare a solution containing Mo, wherein Mo is in the form of MoO 3 The weight concentration of the sodium aluminate solution was 32 g / L, and it was divided into 5 equal parts by volume. The Al in the sodium aluminate solution accounted for 1.3% of the total Al (in terms of Al) in the obtained hydrocracking catalyst. 2 O 3 30% of the total weight of the raw materials (calculated), and divided it into 5 equal parts by volume. Prepare β molecular sieve slurry at a solid-liquid ratio of 1:3, and divide it into 5 equal parts by volume. The solution containing W, Ni, and Al is placed in a reaction tank, the reaction temperature is 60°C, and a mixed solution of 12wt% sodium hydroxide and sodium bicarbonate and ammonia water with a weight concentration of 6% are dripped and added to the reaction tank in parallel for gelation reaction. The molar ratio of sodium hydroxide to sodium bicarbonate is 0.4:1, and the ratio of the molar number of ammonia water to the sum of sodium hydroxide and sodium bicarbonate is 0.25. The initial pH value is controlled to 5.1, and the pH value is increased by 5 times to adjust the final pH value to 9.1 at the end. The pH value increased by 0.8 each time, and each time it is increased to the adjusted value, after , add a portion of molybdenum-containing solution, keep the adjusted pH value of the reaction slurry constant for 12 minutes, generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum, and age the resulting slurry at an aging temperature of 76°C. During aging, add an equal portion of sodium aluminate solution to control the pH value to 13.3, add an equal portion of β molecular sieve slurry, and after aging for 0.15 hours, control the aging pH value to 9.4, and after aging for 0.2 hours, then control the pH value to 5.5, and the aging time is 0.15 hours. Repeat the above operation process 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The molded product is dried at 100°C for 8.0 hours, and the dried material is roasted at 530°C for 5 hours to obtain catalyst A. The catalyst composition and main properties are shown in Table 1.

[0044] Example 2

[0045] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. In the solution containing W, Ni and Al, W is WO 3 The weight concentration of Ni as NiO is 44 g / L, the weight concentration of Al as Al is 52 g / L. 2 O 3 The weight concentration is 29.9 g / L. Ammonium molybdate is added to the dissolution tank 2 filled with deionized water to prepare a solution containing Mo, wherein Mo is in the form of MoO 3 The weight concentration of the sodium aluminate solution was 36 g / L, and it was divided into 6 equal parts by volume. The Al in the sodium aluminate solution accounted for 1.3% of the total Al (in terms of Al) in the obtained hydrocracking catalyst. 2 O3 35% of the total weight of the raw materials (calculated), and divided it into 5 equal parts by volume. Prepare β molecular sieve slurry at a solid-liquid ratio of 1:3.8, and divide it into 5 equal parts by volume. The solution containing W, Ni, and Al is placed in a reaction tank, the reaction temperature is 55°C, and a mixed solution of 13wt% sodium hydroxide and sodium bicarbonate and ammonia water with a weight concentration of 7% are dripped and added to the reaction tank in parallel for gelation reaction. The molar ratio of sodium hydroxide to sodium bicarbonate is 0.5:1, and the ratio of the molar number of ammonia water to the sum of sodium hydroxide and sodium bicarbonate is 0.29. The initial pH value is controlled to 5.6, and the final pH value at the end is adjusted to 9.8 by increasing the pH value 6 times. The pH value increased by 0.7 each time, and each time it is increased to the adjusted value, after , add a portion of molybdenum-containing solution, keep the adjusted pH value of the reaction slurry constant for 14 minutes, generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum, and age the resulting slurry at an aging temperature of 80°C. During aging, add an equal portion of sodium aluminate solution to control the pH value to 13.0, add an equal portion of β molecular sieve slurry, and after aging for 0.2 hours, control the aging pH value to 9.0, and after aging for 0.15 hours, then control the pH value to 5.0, and the aging time is 0.15 hours. Repeat the above operation process 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 100°C for 10 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The molded product is dried at 90°C for 8.0 hours, and the dried material is roasted at 540°C for 4 hours to obtain catalyst B. The catalyst composition and main properties are shown in Table 1.

[0046] Example 3

[0047] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. In the solution containing W, Ni and Al, W is WO 3 The weight concentration of Ni as NiO is 40g / L, the weight concentration of Al as Al is 60g / L. 2 O 3 The weight concentration is 34.5 g / L. Ammonium molybdate is added to the dissolution tank 2 filled with deionized water to prepare a solution containing Mo, wherein Mo is in the form of MoO 3 The weight concentration of the sodium aluminate solution was 30 g / L, and it was divided into 4 equal parts by volume. The Al in the sodium aluminate solution accounted for 1.3% of the total Al (in terms of Al) in the obtained hydrocracking catalyst. 2 O 325% of the total weight of the raw materials (calculated), and divided it into 6 equal parts by volume. Prepare β molecular sieve slurry at a solid-liquid ratio of 1:3.5, and divide it into 6 equal parts by volume. The solution containing W, Ni, and Al is placed in a reaction tank, the reaction temperature is 65°C, and a mixed solution of 14wt% sodium hydroxide and sodium bicarbonate and ammonia water with a weight concentration of 5% are dripped and added to the reaction tank in parallel for gelation reaction. The molar ratio of sodium hydroxide to sodium bicarbonate is 0.45:1, and the ratio of the molar number of ammonia water to the sum of sodium hydroxide and sodium bicarbonate is 0.38. The initial pH value is controlled to 5.3, and the final pH value at the end is adjusted to 8.9 by increasing the pH value 4 times. The pH value increased by 0.9 each time, and the pH value increased by 4 times to the adjusted value each time. After that, a portion of molybdenum-containing solution was added, and the pH value of the adjusted reaction slurry was kept constant for 11 minutes to generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum. The resulting slurry was aged at an aging temperature of 85°C. During aging, an equal portion of sodium aluminate solution was first added to control the pH value to 12.8, and an equal portion of β molecular sieve slurry was added. After aging for 0.2 hours, the aging pH value was controlled at 9.6. After aging for 0.2 hours, the pH value was then controlled to 5.3, and the aging time was 0.15 hours. The above operation process was repeated 6 times to end aging. The aged slurry was filtered, the filter cake was dried at 110°C for 7 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The molded product was dried at 80°C for 9.0 hours, and the dried material was calcined at 500°C for 5 hours to obtain catalyst C. The catalyst composition and main properties are shown in Table 1.

[0048] Example 4

[0049] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. In the solution containing W, Ni and Al, W is WO 3 The weight concentration of Ni as NiO is 50 g / L, the weight concentration of Al as Al is 40 g / L. 2 O 3 The weight concentration is 32.6 g / L. Ammonium molybdate is added to the dissolution tank 2 filled with deionized water to prepare a solution containing Mo, wherein Mo is in the form of MoO 3 The weight concentration of the sodium aluminate solution was 40 g / L, and it was divided into 7 equal parts by volume. The Al in the sodium aluminate solution accounted for 1.3% of the total Al (in terms of Al) in the obtained hydrocracking catalyst. 2 O 332% of the total weight of the raw materials (calculated), and divided it into 4 equal parts by volume. Prepare β molecular sieve slurry at a solid-liquid ratio of 1:2.8, and divide it into 4 equal parts by volume. The solution containing W, Ni, and Al is placed in a reaction tank, the reaction temperature is 68°C, and a mixed solution of 11wt% sodium hydroxide and sodium bicarbonate and ammonia water with a weight concentration of 7% are dripped and added to the reaction tank in parallel for gelation reaction. The molar ratio of sodium hydroxide to sodium bicarbonate is 0.52:1, and the ratio of the molar number of ammonia water to the sum of sodium hydroxide and sodium bicarbonate is 0.30. The initial pH value is controlled to 5.1, and the pH value is increased by 7 times to adjust the final pH value to 10.0 at the end. The pH value increased by 0.7 each time, and the pH value was increased to the adjustment value each time. After that, a portion of molybdenum-containing solution was added, and the pH value of the adjusted reaction slurry was kept constant for 14 minutes to generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum. The resulting slurry was aged at an aging temperature of 82°C. During aging, an equal portion of sodium aluminate solution was first added to control the pH value to 13.0, and an equal portion of β molecular sieve slurry was added. After aging for 0.2 hours, the aging pH value was controlled at 9.6. After aging for 0.15 hours, the pH value was then controlled to 5.1, and the aging time was 0.15 hours. The above operation process was repeated 4 times to end aging. The aged slurry was filtered, the filter cake was dried at 90°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The molded product was dried at 80°C for 10.0 hours, and the dried material was roasted at 510°C for 4 hours to obtain catalyst A. The catalyst composition and main properties are shown in Table 1.

[0050] Comparative Example 1

[0051] Reference catalyst E was prepared according to the method disclosed in CN101239324A. The components and active metal content were the same as those in Example 1. The molecular sieve was β molecular sieve. The specific steps were as follows: (1) nickel chloride, ammonium molybdate, and aluminum chloride solution were added to a dissolution tank filled with deionized water. The mass concentration of Ni in the solution was 52 g / L in terms of NiO, and the mass concentration of Mo in the solution was 52 g / L in terms of MoO. 3 The weight concentration of Al is 32g / L. 2 O 3 The mass concentration is 22g / L, and 2000mL of clean water is added to dilute; (2) Ammonia water is added while stirring until the pH value is 5.2; (3) Sodium tungstate solution containing WO 3The reaction mixture was stirred at 40 °C for 1 h and the reaction mixture was stirred at 50 °C for 2 h. The reaction mixture was stirred at 40 °C for 3 h. The reaction mixture was stirred at 50 °C for 1 h. The reaction mixture was stirred at 50 °C for 2 h. The reaction mixture was stirred at 50 °C for 3 h. The reaction mixture was stirred at 50 °C for 2 h. The reaction mixture was stirred at 50 °C for 3 h. The reaction mixture was stirred at 50 °C for 4 h. The reaction mixture was stirred at 50 °C for 2 h. The reaction mixture was stirred at 50 °C for 3 h. The reaction mixture was stirred at 50 °C for 3 h. The reaction mixture was stirred at 50 °C for 4 h. The reaction mixture was stirred at 50 °C for 2 h. The reaction mixture was stirred at 50 °C for 3 h.

[0052] Comparative Example 2

[0053] According to the preparation method disclosed in CN106179462A, a reference agent F having the same catalyst composition as Example 1 of the present invention was prepared, wherein the acidic component was β molecular sieve, and the specific process was as follows:

[0054] Nickel chloride and aluminum chloride solutions were dissolved in deionized water to prepare mixed solution A. The weight concentration of NiO in mixed solution A was 52 g / L, and the weight concentration of Al 2 O 3 The weight concentration is 15.4 g / L. Dissolve ammonium metatungstate, ammonium molybdate and aluminum chloride solution in deionized water to prepare mixed solution B. 3 The weight concentration is 68g / L, MoO 3 The weight concentration is 32g / L, Al 2 O 3The weight concentration is 6.6 g / L. Ammonia water with a concentration of 10% (weight) is added to solution A under stirring, the gelling temperature is maintained at 62°C, the pH value is controlled at 7.8 at the end, and the gelling time is controlled at 0.8 hours to generate nickel and aluminum precipitate slurry I. Deionized water is added to the reaction tank, and ammonia water with a concentration of 10% (weight) and solution B are added to the reaction tank in parallel, the gelling temperature is maintained at 62°C, the pH value is controlled at 7.8 during the parallel gelling reaction, and the gelling time is controlled at 1.0 hours to generate tungsten, molybdenum, and aluminum precipitate slurry II. The two precipitate-containing slurries were mixed and aged for 4.0 hours at 78°C and pH value was controlled at 7.6. The mixture was then filtered and the filter cake was hydrothermally treated under water vapor containing urea. The conditions for the hydrothermal treatment were as follows: the molar ratio of urea to the total amount of active metal atoms was 7:1, the temperature was 250°C, the pressure was 4.0MPa, and the treatment time was 3 hours. After the treatment, the filter cake was slurried and the β molecular sieve suspension was stirred evenly in the mixture slurry. The filter cake was dried at 100°C for 9 hours, rolled, and extruded. Wash with deionized water at room temperature until neutral. The washed wet strips were then dried at 80°C for 10.0 hours. The dried material was calcined at 540°C for 4 hours to obtain catalyst F. The catalyst composition, pore distribution and main properties are shown in Table 1.

[0055] Comparative Example 3

[0056] The reference agent G is prepared in the same manner as Example 1 of this patent, except that the acidic component is Y molecular sieve. The catalyst composition and main properties are shown in Table 1.

[0057] Comparative Example 4

[0058] The same as Example 1, the reference agent H was prepared, and all the sodium aluminate solution and the β molecular sieve slurry were added at one time during the aging process of the precipitate slurry containing nickel, molybdenum, tungsten and aluminum, and the aging pH value was fixed. The specific preparation process is as follows:

[0059] Ammonium metatungstate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni and Al. In the solution containing W, Ni and Al, W is WO 3 The weight concentration of Ni as NiO is 58g / L, the weight concentration of Al as Al is 44g / L. 2 O 3 The weight concentration is 28 g / L. Ammonium molybdate is added to the dissolution tank 2 filled with deionized water to prepare a solution containing Mo, wherein Mo is in the form of MoO 3 The weight concentration of the sodium aluminate solution was 32 g / L, and it was divided into 5 equal parts by volume. The Al in the sodium aluminate solution accounted for 1.3% of the total Al (in terms of Al) in the obtained hydrocracking catalyst. 2 O 3The solution containing W, Ni and Al is put into a reaction tank, and a mixed solution of sodium hydroxide and sodium bicarbonate with a concentration of 12wt% and ammonia water with a weight concentration of 6% are dripped into the reaction tank and added to the reaction tank for gelling reaction. The molar ratio of sodium hydroxide to sodium bicarbonate is 0.4:1, and the ratio of the molar number of ammonia water to the sum of the moles of sodium hydroxide and sodium bicarbonate is 0.25. The initial pH value is controlled to be 5.1, and the pH value is adjusted up 5 times to adjust the final pH value to 9.1 at the end. The pH value is adjusted up to 0.8 each time. After each adjustment to the adjusted value, a portion of molybdenum-containing solution is added, and the pH value of the adjusted reaction slurry is kept constant for 12 minutes to generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum. The obtained slurry is aged. At the beginning of aging, all the sodium aluminate solution and β molecular sieve slurry are added. The aging temperature is 76°C, the pH value is controlled at 8.0, the aging time is 2.5 hours, and the aging is terminated. The aged slurry was filtered, the filter cake was dried at 100°C for 8 hours, rolled, and extruded into strips. The shaped material was washed with deionized water at room temperature until neutral. The shaped material was dried at 100°C for 8.0 hours, and the dried material was calcined at 530°C for 5 hours to obtain catalyst H. The catalyst composition and main properties are shown in Table 1.

[0060] Comparative Example 5

[0061] The reference agent I was prepared in the same manner as in Example 1. In the preparation process, W, Ni, Mo, and Al solutions were directly prepared to participate in the gelling reaction. The gelling reaction was carried out at a fixed pH value. The specific preparation process is as follows:

[0062] Ammonium metatungstate, ammonium molybdate, nickel chloride and aluminum chloride are added to a dissolving tank 1 filled with deionized water to prepare a solution containing W, Ni, Mo and Al. 3 The weight concentration of Ni as NiO is 58 g / L, the weight concentration of Mo as MoO 3 The weight concentration of Al is 32g / L. 2 O 3 The weight concentration of the sodium aluminate solution is 28 g / L. The Al in the sodium aluminate solution accounts for 1.3% of the total Al in the hydrocracking catalyst (measured as Al 2 O 330% of the total weight of the raw materials (calculated), and divided it into 5 equal parts by volume. Prepare β molecular sieve slurry at a solid-liquid ratio of 1:3, and divide it into 5 equal parts by volume. Put the solution containing W, Mo, Ni, and Al into a reaction tank, and drop a mixed solution of sodium hydroxide and sodium bicarbonate with a concentration of 12wt% and ammonia water with a weight concentration of 6% into the reaction tank for gelation reaction. The molar ratio of sodium hydroxide to sodium bicarbonate is 0.4:1, and the ratio of the molar number of ammonia water to the sum of sodium hydroxide and sodium bicarbonate is 0.25. The initial pH value is controlled to 5.1, and the final pH value is adjusted to 9.1 at the end by increasing the pH value 5 times. The pH value is increased by 0.8 each time, and the pH value is adjusted each time. After the pH value is adjusted, the adjusted reaction slurry pH value is kept constant for 12 minutes to generate a precipitate slurry containing nickel, molybdenum, tungsten and aluminum. The resulting slurry is aged at an aging temperature of 76°C. During aging, an equal portion of sodium aluminate solution is first added to control the pH value to 13.3, and an equal portion of β molecular sieve slurry is added. After aging for 0.15 hours, the aging pH value is controlled at 9.4. After aging for 0.2 hours, the pH value is then controlled to 5.5, and the aging time is 0.15 hours. Repeat the above operation process 5 times to end aging. The aged slurry is filtered, the filter cake is dried at 100°C for 8 hours, rolled, and extruded into strips. Wash with deionized water at room temperature until neutral. The molded product is dried at 100°C for 8.0 hours, and the dried material is roasted at 530°C for 5 hours to obtain catalyst I. The catalyst composition and main properties are shown in Table 1.

[0063] Comparative Example 6

[0064] Similar to Example 1, the precipitation reaction was carried out using precipitant A to prepare reference agent J.

[0065] Comparative Example 7

[0066] The same method as in Example 1 was used to carry out precipitation reaction using precipitant B to prepare reference agent K.

[0067] Example 5

[0068] This example is an activity evaluation experiment of the catalyst of the present invention, and is compared with the catalyst of the comparative example. The catalysts A, B, C, D of the present invention and the catalysts E, F, G, H, I, J, K of the comparative example are respectively used to conduct comparative evaluation tests on a 200mL small hydrogenation device, and the comparative evaluation tests are conducted on a 200mL small hydrogenation device. The evaluation conditions are: total reaction pressure 15.7MPa, hydrogen-oil volume ratio 1200:1, liquid hourly volume space velocity 1.6h -1, reaction temperature 375 ℃, 385 ℃, the raw material for evaluation is vacuum wax oil, its main properties are shown in Table 4, and the evaluation results are shown in Tables 5-6. It can be seen from Tables 1-3 that the average particle size of the catalyst oxide particles of the present invention is small and evenly distributed, there are many surface active metals, the pore size is concentrated in 6-10nm, and there is a good synergistic effect between the acidic component and the hydrogenation component. It can be seen from the evaluation results that compared with the comparative example catalyst, the active metal distribution, pore size distribution and average particle size of the catalyst of the present invention are all conducive to improving the aromatic saturation performance. The catalyst of the present invention has both high isomerization performance and high aromatic saturation performance in the hydrocracking process of heavy raw oil, and can produce No. 5 industrial grade white oil and lubricating oil base oil. The comparative example catalyst cannot have high isomerization performance and high aromatic saturation performance at the same time. The hydrocracking catalyst of the present invention still has good stability and good product quality under high nitrogen content feed conditions.

[0069] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples

[0070] Catalyst No. A B C D E F NiO, wt% 22 26 30 20 26 26 <![CDATA[WO 3 ,wt%]]> 29 22 20 25 34 34 <![CDATA[MoO 3 ,wt%]]> 16 18 15 20 16 16 <![CDATA[Al 2 O 3 ,wt%]]> 20 23 23 24 11 11 <![CDATA[SiO 2 ,wt%]]> 13 11 12 11 13 13 <![CDATA[Specific surface area, m 2 / g]]> 446 438 454 458 228 377 Pore ​​volume, mL / g 0.481 0.473 0.492 0.499 0.323 0.410 Pore ​​distribution <6nm 6.14 6.92 5.12 4.63 62.47 35.16 6nm~10nm 65.15 65.01 65.80 65.34 18.54 35.14 10nm~15nm 15.32 15.04 14.86 15.42 10.51 16.02 >15nm 13.39 13.03 14.22 14.61 8.48 13.68

[0071] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples

[0072]

[0073]

[0074] Table 2 Ratio of the weight content of active metal oxides on the catalyst surface to the weight content of active metal oxides in the bulk phase

[0075] Catalyst No. A B C D E F <![CDATA[Surface I W+Ni / Bulk I W+Ni > 5.11 5.03 5.45 5.57 0.92 1.02 <![CDATA[Surface I Mo + Ni / Bulk I Mo + Ni > 4.21 4.14 4.36 4.48 1.03 0.99

[0076] Table 2

[0077] Catalyst No. G H I J K <![CDATA[Surface I W+Ni / Bulk I W+Ni > 5.04 3.22 3.38 1.09 0.96 <![CDATA[Surface I Mo+Ni / Bulk I Mo+Ni > 4.16 1.75 1.89 1.05 0.90

[0078] Table 3 Average particle size and particle size distribution of the catalyst oxide particles obtained in each example

[0079]

[0080]

[0081] Table 3 Average particle size and particle size distribution of the catalyst oxide particles obtained in each example

[0082] Catalyst No. G H I J K Average particle size of oxide particles, nm 10.1 19.5 17.1 15.9 30.1 Oxide particle size distribution, % Particle size less than 8nm 8.41 8.91 7.51 47.23 1.64 Particle size is 8nm-12nm 79.98 25.45 29.42 20.98 5.18 Particle size greater than 12nm 11.61 65.64 63.07 31.79 93.18

[0083] Table 4 Main properties of crude oil

[0084]

[0085] Table 5 Evaluation results of catalysts of Examples and Comparative Examples (operation for 250 hours)

[0086]

[0087]

[0088] Table 5 Evaluation results of catalysts of Examples and Comparative Examples (operation for 250 hours)

[0089] catalyst G H I J K Reaction temperature, °C 375 375 375 375 375 Nitrogen content in feed, μg / g 118 118 118 118 118 82~132℃ heavy naphtha Aromatic potential, wt% 58.6 60.8 60.5 60.2 59.5 132~282℃ Aviation fuel Smoke point / mm 29.6 25.1 25.3 23.0 23.5 Aromatics, v% 1.7 12.5 12.4 18.8 17.3 282~370℃ diesel Pour point / ℃ 3 -8 -7 -8 -8 Aromatics / wt% 2.0 12.6 10.8 14.0 12.9 >370℃ tail oil BMCI value 5.4 14.4 15.8 24.1 23.4 Viscosity Index 123 103 105 92 96

[0090] Table 6 Evaluation results of catalysts of Examples and Comparative Examples (operation 2000 hours)

[0091]

[0092]

[0093] Table 7 Properties of β molecular sieves in Examples and Comparative Examples

[0094] Silicon to aluminum molar ratio 80.5 <![CDATA[Specific surface area, m 2 / g]]> 621 Pore ​​volume, mL / g 0.55 IR total acid, mmol / g 0.43 <![CDATA[Na 2 O,wt%]]> 0.080

[0095] Table 8 Properties of Y-type molecular sieve used in the present invention

[0096]

[0097]

Claims

1. A method for preparing a bulk hydrocracking catalyst, characterized in that The method comprises the following contents: (1) adding a solution containing W, Ni and Al into a gelling reaction tank, and dripping a precipitant A and a precipitant B into the reaction tank in parallel to perform a gelling reaction; during the gelling reaction, the pH value is controlled by the precipitant to increase from an initial value to a final value, and a molybdenum-containing solution is added after each increase; the number of increments n is 2 to 10 times, preferably 2 to 8 times; (2) the slurry obtained in step (1) is aged n times continuously, and 1 / n sodium aluminate solution and 1 / n β molecular sieve slurry are added during each aging process, and the mixture is evenly mixed; the slurry obtained after aging is filtered to obtain a solid phase material; Each aging process adopts a pH value gradually decreasing aging process; (3) the solid phase material obtained in step (2) is dried, formed, washed, and then dried and calcined to obtain a hydrocracking catalyst; wherein the precipitant A described in step (1) is a mixed solution of sodium hydroxide and sodium bicarbonate, and the precipitant B is ammonia water.

2. The method according to claim 1, characterized in that: In the W, Ni and Al solution described in step (1), the weight concentration of W calculated as WO3 is 5 to 140 g / L, the weight concentration of Ni calculated as NiO is 5 to 130 g / L, and the weight concentration of Al calculated as Al2O3 is 2 to 90 g / L.

3. The method according to claim 1, characterized in that: The concentration of the mixed solution of sodium hydroxide and sodium bicarbonate described in step (1) is 7wt% to 20wt%, the molar ratio of sodium hydroxide to sodium bicarbonate is 0.2:1 to 0.8:1, preferably 0.3:1 to 0.7:1, the concentration of ammonia water is 4wt% to 8wt%, and the molar ratio of ammonia water to the mixed solution of sodium hydroxide and sodium bicarbonate is 0.1:1 to 0.45:1, preferably 0.15:1 to 0.40:

1.

4. The method according to claim 1, characterized in that: When the gelling reaction in step (1) starts, the initial pH value is controlled to be 5.0-6.5, and the time required is 0.05-0.4 hours; the final pH value is 8.0-10.5, the gelling reaction temperature is 40-90°C, and the gelling reaction time is 0.3-5.0 hours.

5. The method according to claim 1, characterized in that: During the gelling reaction described in step (1), the pH value is kept constant for 0.05 to 0.5 hours after each increase, and the increase in pH value each time is not greater than the increase in pH value of the previous time.

6. The method according to claim 1, characterized in that: In the Mo-containing solution described in step (1), the weight concentration of Mo in terms of MoO3 is 10 to 150 g / L, preferably 10 to 140 g / L; the molybdenum-containing solution is added in batches according to the increasing number of pH values, and the volume of the molybdenum-containing solution added each time is the same or different, and the total amount of the molybdenum-containing solution is determined according to the catalyst composition.

7. The method according to claim 1, characterized in that: The sodium aluminate solution described in step (2) has a weight concentration of 5 to 75 g / L in terms of Al2O3; the sodium aluminate solution is divided into 2 to 8 portions by volume according to the number of additions, preferably divided equally by volume; The β molecular sieve slurry is divided into 2 to 8 portions by volume according to the number of additions, preferably divided equally by volume.

8. The method according to claim 1, characterized in that: The aging temperature in step (2) is 60 to 98°C, preferably 65 to 92°C.

9. The method according to claim 1, characterized in that: The pH value of the step-by-step decreasing aging process described in step (2) is as follows: the reaction slurry is dripped into a 1 / n sodium aluminate solution to adjust the pH value, the pH value is controlled at 11.5-13.5, 1 / n β molecular sieve slurry is added, and the aging is performed for 0.05-0.5 hours; then the pH value is adjusted to 8.5-10.5, and the aging time is 0.05-0.5 hours; finally, the pH value is adjusted to 4.0-6.5, and the aging time is 0.05-0.5 hours, wherein n is an integer of 2-8.

10. The method according to claim 1, characterized in that: In step (2), the Al added to the sodium aluminate solution accounts for 5% to 50% of the total Al in the obtained hydrocracking catalyst calculated as Al2O3.

11. The method according to claim 1, characterized in that: The beta molecular sieve described in step (2) has the following properties: a molar ratio of silicon oxide to aluminum oxide of 30 to 90, a specific surface area of ​​430 to 780 m 2 / g, pore volume is 0.30~0.90cm 3 / g, the infrared acid content is 0.10~0.45mmol / g; the beta molecular sieve slurry is a mixture of beta molecular sieve and deionized water after being stirred evenly, and the solid-liquid mass ratio is 1:1.2~1:

4.

12. A bulk hydrocracking catalyst prepared by the method according to any one of claims 1 to 11, characterized in that: The hydrocracking catalyst comprises a hydrogenation active metal component, amorphous alumina and beta molecular sieve; the pore size distribution of the hydrocracking catalyst is as follows: the pore volume occupied by pores with a diameter of less than 6 nm accounts for 2% to 14% of the total pore volume, the pore volume occupied by pores with a diameter of 6 to 10 nm accounts for 52% to 73% of the total pore volume, the pore volume occupied by pores with a diameter of 10 to 15 nm accounts for 10% to 25% of the total pore volume, and the pore volume occupied by pores with a diameter of more than 15 nm accounts for 6% to 23% of the total pore volume. The molar ratio of W / Mo is 1:13~10:1, preferably 1:11~9:1, and the molar ratio of Ni / (Mo+W) is 1:14~13:1, preferably 1:12~12:1; wherein the ratio of the sum of the weight contents of the surface active metal components WO3 and NiO to the sum of the weight contents of the bulk active metal components WO3 and NiO is 2.4:1~6.5:1, preferably 3.5:1~6.2:1, and the ratio of the sum of the weight contents of the surface active metal components MoO3 and NiO to the sum of the weight contents of the bulk active metal components MoO3 and NiO is 2.3:1~5.6:1, preferably 2.5:1~5.3:

1.

13. A bulk hydrocracking catalyst prepared by the method according to any one of claims 1 to 11, characterized in that: The average particle size of tungsten, molybdenum and nickel active metal oxide particles is 8~12nm; the particle size distribution of tungsten, molybdenum and nickel active metal oxide particles is as follows: the number of particles with a particle size less than 8nm accounts for 3%~15% of the total number of particles, the number of particles with a particle size of 8nm~12nm accounts for 70%~90% of the total number of particles, and the number of particles with a particle size greater than 12nm accounts for 6%~18% of the total number of particles.

14. Use of a bulk hydrocracking catalyst prepared by the method according to any one of claims 1 to 11 in a hydrocracking process of base oil feedstocks of No. 5 industrial grade white oil and high viscosity index lubricating oil.

15. The use according to claim 14, characterized in that: The nitrogen content in the feed of the hydrocracking process is less than 150 μg / g and is above 10 μg / g, preferably above 50 μg / g.

Citation Information

Patent Citations

  • Preparation method of hydrocracking catalyst

    CN103055927A

  • Preparation method of hydro-cracking catalyst

    CN104588083A

  • Preparation method of hydrofining catalyst