Composite catalyst as well as preparation method and application thereof
By introducing phosphorus modification and compounding the second molecular sieve on the ZSM-5 hierarchical pore molecular sieve, combined with the carrier, a composite catalyst is prepared, which solves the problem of low yield of low-carbon olefins caused by the small pore size of the catalyst, and improves the activity and reaction of the catalyst performance, achieving efficient production of low-carbon olefins.
Patent Information
- Application Number
- CN202310333556.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The existing ZSM-5 hierarchical pore molecular sieve has a small pore size in the production of low-carbon olefin catalysts, resulting in unfavorable diffusion and adsorption of macromolecular reactants, low low-carbon olefin yields, and common synthesis routes have special raw materials or template structures. The lack of mesopores prevents wide application.
The phosphorus-containing hollow ZSM-5 hierarchical pore molecular sieve is compounded with the second molecular sieve, combined with the carrier, to prepare a composite catalyst, which improves the accessibility of the catalyst's active center and the diffusion performance of reacting molecules, and is used for hydrogenation of LCO catalytic cracking or heavy oil catalytic cracking. .
It significantly improves the yield of low-carbon olefins, enhances the activity of the catalyst and the diffusion performance of reaction molecules, and solves the shortcomings of existing catalysts in the yield and application range of low-carbon olefins.
Smart Images

Figure CN118767978A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composite catalyst and a preparation method and application thereof. Background Art
[0002] Ethylene and propylene are very important chemical raw materials. At present, the world mainly uses naphtha steam cracking to produce low-carbon olefins. However, the output of naphtha is limited, and the demand for low-carbon olefins in the world is increasing. Therefore, it is of great significance to develop and utilize other raw materials to produce low-carbon olefins.
[0003] In the catalysts for producing light olefins, ZSM-5 molecular sieves with MFI topology and β molecular sieves with BEA topology are usually used. Although ZSM-5 molecular sieves have shape-selective function, their pore size is small, which is not conducive to the diffusion and adsorption of macromolecular reactants, especially cyclic hydrocarbons, resulting in low yield of light olefins. At present, there are many synthetic routes based on ZSM-5 multi-level pore molecular sieve materials, but these methods all have certain shortcomings, such as using special raw materials or templates to construct mesopores, or adding additional raw materials to the gel and removing them after post-treatment, which makes them unable to be widely used. Summary of the invention
[0004] The purpose of the present invention is to provide a composite catalyst and a preparation method and application thereof, so as to significantly improve the yield of light olefins.
[0005] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a composite catalyst, which comprises a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, a second molecular sieve and a carrier, wherein the content of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 5-35% by weight, the content of the second molecular sieve is 10-50% by weight, and the content of the carrier is 30-80% by weight based on the dry weight of the composite catalyst;
[0006] The phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve has a hollow structure, an average grain size of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, a ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the total specific surface area of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 340-400 m 2 / g, mesoporous specific surface area is 40-150m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area; the strong B acid content of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve accounts for 65-80% of the total B acid content, and the strong L acid content accounts for 50-75% of the total L acid content;
[0007] The second molecular sieve is a molecular sieve with a pore size of 0.56-0.75 nm, or the second molecular sieve is a Y-type molecular sieve containing rare earth.
[0008] Optionally, the phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.2-1.3.
[0009] Optionally, the average grain size of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve grains is 0.4-2.5 μm, the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.1-1.4, and the relative crystallinity is 75-90%.
[0010] Optionally, the total specific surface area of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 350-400m 2 / g, mesopore specific surface area is 45-140m 2 / g, and the mesoporous specific surface area accounts for 20-35% of the total specific surface area.
[0011] Optionally, the molecular sieve with a pore size of 0.56-0.75 nm is one or more of the molecular sieves having AET, AFR, AFS, AFI, BEA, BOG, CFI, CON, GME, IFR, ISV, LTL, MEI, MOR, OFF and SAO structures; preferably at least one of Beta, SAPO-5, SAPO-40, SSZ-13, CIT-1, ITQ-7, ZSM-18, mordenite and gmelinite;
[0012] The rare earth content of the Y-type molecular sieve is 2-25% by weight as rare earth element oxide, and the rare earth element is lanthanum and / or cerium; the phosphorus content of the Y-type molecular sieve is 0-10% by weight as P2O5; the Y-type molecular sieve is selected from one or more of REY molecular sieve, DASY molecular sieve, USY molecular sieve, phosphorus-containing DASY molecular sieve, phosphorus-containing USY molecular sieve, PSRY molecular sieve, HRY molecular sieve, HSY molecular sieve, SCY molecular sieve, and RSCY molecular sieve.
[0013] Optionally, the carrier is selected from one or more of natural clay, alumina carrier, silica carrier, aluminum phosphate carrier and silica-alumina carrier;
[0014] Preferably, the silica carrier is one or more of neutral silica sol, acidic silica sol or alkaline silica sol; the alumina carrier is one or more of aluminum sol, acidified pseudo-boehmite, hydrated alumina and activated alumina; the aluminum phosphate carrier is phosphate aluminum gel; the silica aluminum oxide carrier is one or more of solid silica aluminum material, silica aluminum sol and silica aluminum gel.
[0015] Optionally, the carrier comprises a silicon oxide carrier; the content of the silicon oxide carrier in terms of SiO2 is 1-20 wt % based on the dry weight of the composite catalyst.
[0016] The second aspect of the present disclosure provides a method for preparing the composite catalyst described in the first aspect of the present disclosure, the method comprising: subjecting a slurry containing a carrier, a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, a second molecular sieve and water to a first drying and an optional first calcination.
[0017] Optionally, the preparation steps of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve include:
[0018] (1) Mixing a first organosilicon source and a first solvent at 30-50° C. and stirring for 0.5-5 hours, then heating to 70-100° C. and stirring for 2-10 hours, and mixing the obtained mixed liquid with a first template at 20-30° C. for 0.5-3.0 hours to obtain a first mixed product;
[0019] (2) mixing a first alkali metal hydroxide, a second solvent and a first aluminum source, calculated as Al2O3, in a molar ratio of (1.5-5):(60-350):1 at 20-80° C. for 0.5-2.0 hours to obtain a second mixed product;
[0020] (3) mixing the first mixed product and the second mixed product and subjecting them to dynamic crystallization, taking out the obtained solid and subjecting it to a second calcination to obtain a first solid product;
[0021] (4) mixing the first solid product with a first solution containing alkali, heating the mixture to a reaction temperature at a heating rate of 1-5° C. / min, and reacting the mixture at the reaction temperature for 10-90 min to obtain a second solid product; wherein the reaction temperature is 60-90° C., and the content of alkali in the first solution containing alkali is 0.45-2 mol / L;
[0022] (5) subjecting the second solid product to a first ammonium exchange, and optionally a sixth calcination, to obtain a third solid product;
[0023] (6) mixing the third solid product with a second solution containing a phosphorus source, and subjecting the obtained first slurry to a second drying and a third calcination; or,
[0024] The preparation steps of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve include:
[0025] S1, mixing the second template, the second inorganic silicon source and the third solvent at 30-50° C. for 0.5-3.0 hours, and subjecting the obtained third mixed product to a first hydrothermal treatment and a second hydrothermal treatment in sequence to obtain a fourth mixed product; wherein the conditions of the first hydrothermal treatment include: a temperature of 80-150° C. and a time of 1-6 hours; the conditions of the second hydrothermal treatment include: a temperature of 160-180° C. and a time of 4-60 hours;
[0026] S2, mixing a second alkali metal hydroxide, calculated as alkali metal oxide, a fourth solvent, and a second aluminum source, calculated as Al2O3, at a molar ratio of (1.5-5):(60-350):1 at 20-80° C. for 0.5-2.0 hours to obtain a fifth mixed product;
[0027] S3, mixing the fourth mixed product and the fifth mixed product, subjecting the obtained mixture to a third hydrothermal treatment, taking out the obtained solid and subjecting it to a fourth roasting to obtain a fourth solid product;
[0028] S4, mixing the fourth solid product with the third solution containing alkali, raising the temperature to the reaction temperature at a heating rate of 1-5°C / min, and reacting at the reaction temperature for 10-90min to obtain a fifth solid product; wherein the reaction temperature is 60-90°C, and the content of alkali in the third solution containing alkali is 0.45-2mol / L;
[0029] S5, subjecting the fifth solid product to a second ammonium exchange, and optionally a seventh roasting, to obtain a sixth solid product;
[0030] S6. Mixing the sixth solid product with the fourth solution containing a phosphorus source, and subjecting the obtained second slurry to a third drying and a fifth calcination.
[0031] Optionally, the first organic silicon source is selected from one or more of methyl orthosilicate and ethyl orthosilicate;
[0032] The second inorganic silicon source is selected from one or more of silica sol, water glass and solid silica gel;
[0033] The first template agent and the second template agent are each independently selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, n-butylamine and hexamethylenediamine;
[0034] The first aluminum source and the second aluminum source are each independently selected from one or more of sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol;
[0035] The first alkali metal hydroxide and the second alkali metal hydroxide are each independently selected from one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide;
[0036] The first alkali-containing solution and the third alkali-containing solution are each independently selected from one or more of a sodium hydroxide solution, a potassium hydroxide solution, a lithium hydroxide solution and a barium hydroxide solution;
[0037] The phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate.
[0038] Optionally, the molar ratio of the total amount of the first template, the first solvent and the second solvent, the first alkali metal hydroxide, and the first organic silicon source is (0.06-0.55): (10-100): (0.02-1.5): 1; the molar ratio of the first organic silicon source to the first aluminum source is (20-500): 1; wherein the first organic silicon source is calculated as SiO2, the first alkali metal hydroxide is calculated as alkali metal oxide, and the first aluminum source is calculated as Al2O3;
[0039] Preferably, in step (2), the molar ratio of the first alkali metal hydroxide, calculated as alkali metal oxide, the second solvent and the first aluminum source, calculated as Al2O3, is (2-4.5): (80-350): 1;
[0040] Preferably, in step (4), the molar ratio of the first solid product to the first alkali-containing solution is 1:(2-10), the first solid product is calculated as SiO2, and the first alkali-containing solution is calculated as alkali metal oxide; the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the first solid product is 1.2-5.0;
[0041] Preferably, in step (6), the weight ratio of the second solution containing the phosphorus source to the third solid product is 1:(0.5-2.0);
[0042] The molar ratio of the total amount of the second template, the third solvent and the fourth solvent, the amount of the second alkali metal hydroxide and the second inorganic silicon source is (0.06-0.55): (10-100): (0.02-1.5): 1, and the molar ratio of the second inorganic silicon source to the second aluminum source is (20-500): 1; wherein the second inorganic silicon source is calculated as SiO2, the second alkali metal hydroxide is calculated as alkali metal oxide, and the second aluminum source is calculated as Al2O3;
[0043] Preferably, in step S2, the molar ratio of the second alkali metal hydroxide, the fourth solvent and the second aluminum source, calculated as Al2O3, is (2-4.5): (80-350): 1;
[0044] Preferably, in step S4, the molar ratio of the fourth solid product to the third alkali-containing solution is 1:(2-10), the fourth solid product is calculated as SiO2, the third alkali-containing solution is calculated as alkali metal oxide, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the fourth solid product is 1.2-5.0;
[0045] Preferably, in step S6, the weight ratio of the fourth solution containing the phosphorus source to the sixth solid product is 1:(0.5-2.0).
[0046] Optionally, the conditions of the dynamic crystallization include: a temperature of 160-180° C. and a time of 12-60 hours;
[0047] The conditions of the third hydrothermal treatment include: temperature of 160-180°C and time of 12-60 hours;
[0048] The conditions of the second calcination, the third calcination, the fourth calcination and the fifth calcination are independently as follows: a temperature of 400-600° C. and a time of 2-6 hours;
[0049] The conditions of the second drying and the third drying each independently include: a temperature of 90-120° C. and a time of 2-24 hours.
[0050] Optionally, the method further comprises: mixing the catalyst particles obtained by the first drying and the optional first calcination, the ammonium salt and the fifth solvent in a weight ratio of 1:(0.1-1):(5-15) to perform a third ammonium exchange, and optionally washing;
[0051] The conditions of the third ammonium exchange include: temperature of 50-100° C. and time of 0.5-2 hours;
[0052] The ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate.
[0053] In a third aspect of the present disclosure, there is provided use of the composite catalyst described in the first aspect of the present disclosure in increasing the production of light olefins in hydrogenation LCO catalytic cracking or heavy oil catalytic cracking.
[0054] Through the above technical scheme, the present invention adopts a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve and a second molecular sieve as the main active component of the catalyst, so that the catalyst has better accessibility to the active center and diffusion performance to the reaction molecules. Using it in hydrogenation LCO catalytic cracking or heavy oil catalytic cracking can effectively increase the yield of light olefins.
[0055] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0057] Figure 1 is a SEM photograph of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve prepared in Example 1 of the present disclosure;
[0058] Figure 2 is a SEM photograph of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve prepared in Example 2 of the present disclosure;
[0059] Figure 3 is a SEM photograph of the second molecular sieve (β molecular sieve with a pore size of 0.59 nm) in Examples 4-6 of the present disclosure;
[0060] Figure 4 This is a SEM photograph of the second molecular sieve (Y-type molecular sieve) in Examples 7-9 of the present disclosure. DETAILED DESCRIPTION
[0061] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0062] In a first aspect, the present disclosure provides a composite catalyst, which contains a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, a second molecular sieve and a carrier. Based on the dry weight of the composite catalyst, the content of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 5-35% by weight, the content of the second molecular sieve is 10-50% by weight, and the content of the carrier is 30-80% by weight; the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the total specific surface area of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 340-400 m 2 / g, mesoporous specific surface area is 40-150m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area; the strong B acid content of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve accounts for 65-80% of the total B acid content, and the strong L acid content accounts for 50-75% of the total L acid content; the second molecular sieve is a molecular sieve with a pore size of 0.56-0.75nm, or the second molecular sieve is a Y-type molecular sieve containing rare earth.
[0063] The composite catalyst disclosed in the present invention contains a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve. The multi-level pore structure of the composite catalyst enables the catalyst to have better accessibility to active centers and diffusion performance to reaction molecules, and can reduce the secondary conversion of light olefins. The composite catalyst is compounded with a second molecular sieve and used in hydrogenation LCO catalytic cracking or heavy oil catalytic cracking to effectively increase the yield of light olefins.
[0064] In a specific embodiment of the present disclosure, the phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.2-1.3. In the present disclosure, the phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is detected by XRF fluorescence method.
[0065] In a specific embodiment of the present disclosure, the average grain size of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve grains is 0.4-2.5μm, preferably 0.6-2.5μm, the ratio of the bulk silicon-aluminum molar ratio (in terms of SiO2 / Al2O3) to the surface silicon-aluminum molar ratio (in terms of SiO2 / Al2O3) is 1.1-1.4, and the relative crystallinity is 75-90%. In the present disclosure, the grain size refers to the size of the widest part of the grain, which can be obtained by measuring the size of the widest part of the grain projection surface in the SEM or TEM image of the sample, and the average grain size is obtained by selecting any 10 molecular sieves in the SEM or TEM image and calculating the average value thereof. The bulk silicon-aluminum molar ratio refers to the silicon-aluminum molar ratio of the entire ZSM-5 nanocrystalline material, which is determined by the XRF method, and the surface silicon-aluminum molar ratio is determined by the XPS method. The specific test method is well known to those skilled in the art and will not be repeated here. The bulk silicon-aluminum molar ratio is 15-200. In the present disclosure, the relative crystallinity of the molecular sieve is based on the XRD standard ZSM-5 molecular sieve standard sample of the China Petroleum and Chemical Research Institute, and the crystallinity of the standard sample is regarded as 100%.
[0066] In a specific embodiment of the present disclosure, the total specific surface area of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve before phosphorus modification is 350-400m 2 / g, mesopore specific surface area is 45-140m 2 / g, the mesopore specific surface area accounts for 20-35% of the total specific surface area, and the N2 adsorption-desorption curve presents an H4-type hysteresis loop. In the present disclosure, the total specific surface area and the mesopore specific surface area are obtained by BET analysis.
[0067] In a specific embodiment of the present disclosure, the strong B acid content accounts for 70-80% of the total B acid content, and the strong L acid content accounts for 55-70% of the total L acid content. The strong B acid content and the total B acid content are prepared by a pyridine infrared acid method, and the strong L acid content and the total L acid content are prepared by a pyridine infrared acid method.
[0068] According to the present disclosure, the molecular sieve having a pore size of 0.56-0.75 nm may be one or more of the molecular sieves having AET, AFR, AFS, AFI, BEA, BOG, CFI, CON, GME, IFR, ISV, LTL, MEI, MOR, OFF and SAO structures; preferably at least one of Beta, SAPO-5, SAPO-40, SSZ-13, CIT-1, ITQ-7, ZSM-18, mordenite and gmelinite.
[0069] According to the present disclosure, the Y-type molecular sieve can be a Y-type molecular sieve that is hydrothermally ultra-stable or gas-phase ultra-stable. The rare earth content of the Y-type molecular sieve is 2-25% by weight in terms of rare earth element oxide (RE2O3), and the rare earth element can be lanthanum and / or cerium; the Y-type molecular sieve can be phosphorus-containing or phosphorus-free, specifically, the phosphorus content of the Y-type molecular sieve is 0-10% by weight in terms of P2O5; the Y-type molecular sieve can be selected from one or more of REY molecular sieve, DASY molecular sieve, USY molecular sieve, phosphorus-containing DASY molecular sieve, phosphorus-containing USY molecular sieve, PSRY molecular sieve, HRY molecular sieve, HSY molecular sieve, SCY molecular sieve, and RSCY molecular sieve.
[0070] According to the present disclosure, the carrier is selected from one or more of natural clay, alumina carrier, silica carrier, aluminum phosphate carrier and silica-alumina oxide carrier. In one embodiment, the silica carrier is one or more of neutral silica sol, acidic silica sol or alkaline silica sol; the alumina carrier is one or more of aluminum sol, acidified pseudo-boehmite, hydrated alumina and activated alumina; the aluminum phosphate carrier is phosphate aluminum gel; the silica-alumina oxide carrier is one or more of solid silica-alumina material, silica-alumina sol and silica-alumina gel.
[0071] In a specific embodiment of the present disclosure, the carrier comprises a silicon oxide carrier; based on the dry weight of the composite catalyst, the content of the silicon oxide carrier in terms of SiO2 is 1-20 wt%.
[0072] In a specific embodiment of the present disclosure, based on the dry weight of the composite catalyst, the composite catalyst contains 20-35 wt% of phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, 10-20 wt% of molecular sieve with a pore size of 0.56-0.75 nm, 20-60 wt% such as 25-50 wt% of clay, 5-35 wt% such as 10-30 wt% of acidified pseudo-boehmite, 3-25 wt% such as 5-15 wt% or 3-20 wt% of aluminum sol and 0-15 wt% such as 3-10 wt% or 5-15 wt% of silica sol.
[0073] In a specific embodiment of the present disclosure, based on the dry weight of the catalyst, the composite catalyst contains 5-20 wt% of a phosphorus-containing hollow ZSM-5 multi-level porous molecular sieve, 15-50 wt% of a rare earth-containing Y-type molecular sieve, 20-60 wt% such as 25-50 wt% of clay, 5-35 wt% such as 10-30 wt% of acidified pseudo-boehmite, 3-25 wt% such as 5-15 wt% or 3-20 wt% of aluminum sol and 0-15 wt% such as 3-10 wt% or 5-15 wt% of silica sol.
[0074] In a specific embodiment of the present disclosure, based on the dry weight of the composite catalyst, the content of sodium oxide in the composite catalyst is preferably 0.15 wt % or less.
[0075] The second aspect of the present disclosure provides a method for preparing the composite catalyst provided by the first aspect of the present disclosure, the method comprising: subjecting a slurry containing a carrier, a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, a second molecular sieve and water to a first drying and an optional first calcination.
[0076] The present disclosure does not limit the specific form of the first drying, which can be conventionally adopted by those skilled in the art. In a preferred embodiment, the first drying is spray drying, which can have a molding effect on the catalyst while drying the material. Spray drying is well known to those skilled in the art, and the specific method is not repeated here.
[0077] In a specific embodiment of the present disclosure, the preparation steps of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve include: (1) mixing a first organic silicon source and a first solvent at 30-50°C for 0.5-5 hours, then heating to 70-100°C and mixing for 2-10 hours, mixing the obtained mixed liquid with a first template at 20-30°C for 0.5-3.0 hours to obtain a first mixed product; (2) mixing a first alkali metal hydroxide, a second solvent and a first aluminum source, calculated as Al2O3, in a molar ratio of (1.5-5): (60-350): 1 at 20-80°C for 0.5-2.0 hours to obtain a second mixed product; (3) mixing the first The mixed product is mixed with the second mixed product and then subjected to dynamic crystallization. The obtained solid is taken out and subjected to a second roasting to obtain a first solid product; (4) the first solid product is mixed with a first solution containing alkali, the temperature is raised to a reaction temperature at a heating rate of 1-5°C / min, and the mixture is reacted at the reaction temperature for 10-90min to obtain a second solid product; wherein the reaction temperature is 60-90°C, and the content of alkali in the first solution containing alkali is 0.45-2mol / L; (5) the second solid product is subjected to a first ammonium exchange to obtain a third solid product; (6) the third solid product is mixed with a second solution containing a phosphorus source, and the obtained first slurry is subjected to a second drying and a third roasting.
[0078] According to the present disclosure, the total amount of the first template, the first solvent and the second solvent, the molar ratio of the first alkali metal hydroxide and the first organic silicon source can vary in a large range, for example, it can be (0.06-0.55): (10-100): (0.02-1.5): 1, preferably (0.08-0.50): (15-85): (0.03-1.2): 1, and the molar ratio of the first organic silicon source to the first aluminum source can be (20-500): 1, preferably (23-200): 1; wherein the first organic silicon source is calculated as SiO2, the first alkali metal hydroxide is calculated as alkali metal oxide (for example, when the first alkali metal hydroxide is NaOH, the first alkali metal hydroxide is calculated as Na2O), and the first aluminum source is calculated as Al2O3. In one embodiment, the first template and the first alkali metal hydroxide contain OH - The ratio of the total molar amount of to the molar amount of the first organic silicon source calculated as SiO2 is (0.01-1.5):1, preferably (0.02-1.2):1.
[0079] According to the present disclosure, in step (2), the molar ratio of the first alkali metal hydroxide, calculated as alkali metal oxide, the second solvent and the first aluminum source, calculated as Al2O3, is preferably (2.0-4.5): (80-350): 1.
[0080] According to the present disclosure, in step (3), dynamic crystallization is well known to those skilled in the art, and the conditions of the dynamic crystallization may include: a temperature of 80-200°C and a time of 4-80 hours; preferably, a temperature of 160-180°C and a time of 12-60 hours.
[0081] According to the present disclosure, in step (4), the weight ratio of the first solid product to the first alkali-containing solution can be 1:(2-10); the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the first solid product is 1.2-5.0.
[0082] According to the present disclosure, in step (5), the first ammonium exchange of the second solid product comprises: mixing the second solid product, the first ammonium source and the fifth solvent in a weight ratio of 1: (0.5-2.0): (5-20), and reacting the obtained mixture at 50-100°C, preferably 60-90°C for 0.5-2 hours. The first ammonium source is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate. The ammonium exchange can be performed once or multiple times. Optionally, the product obtained by the first ammonium exchange is filtered, washed and dried; optionally, the product obtained by the first ammonium exchange is subjected to a sixth roasting, preferably, the product obtained by the first ammonium exchange is subjected to a sixth roasting after being filtered, washed and dried; the temperature of the sixth roasting can be 400-600°C, and the time can be 1-24 hours, preferably 1-10 hours or 1.5-6 hours, more preferably, the temperature is 450-580°C, and the time is 2-4.5 hours.
[0083] According to the present disclosure, in step (6), the weight ratio of the second solution containing the phosphorus source to the third solid product can be 1:(0.5-2.0). The mass content of the phosphorus source in the second solution is, for example, 1-10%.
[0084] According to the present disclosure, compared with the first solid product, the mesopore specific surface area of the hollow ZSM-5 multi-level pore molecular sieve (the third solid product) increases by 100-500%, the mesopore volume increases by 150-600%, and the total acid content increases by 50-250%.
[0085] In another specific embodiment of the present disclosure, the preparation steps of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve include: S1, mixing a second template, a second inorganic silicon source and a third solvent at 30-50°C for 0.5-3.0 hours, and subjecting the obtained third mixed product to a first hydrothermal treatment and a second hydrothermal treatment in sequence to obtain a fourth mixed product; wherein the conditions of the first hydrothermal treatment include: a temperature of 80-150°C and a time of 1-6 hours; the conditions of the second hydrothermal treatment include: a temperature of 160-180°C and a time of 4-60 hours; S2, mixing a second alkali metal hydroxide in terms of alkali metal oxide, a fourth solvent and a second aluminum source in terms of Al2O3 in a molar ratio of (1.5-5): (60-350): 1 at 20-80°C for 0.5-2. 0 hours to obtain a fifth mixed product; S3, mixing the fourth mixed product and the fifth mixed product, subjecting the obtained mixture to a third hydrothermal treatment, taking out the obtained solid and subjecting it to a fourth roasting to obtain a fourth solid product; S4, mixing the fourth solid product with a third solution containing alkali, heating the temperature to the reaction temperature at a heating rate of 1-5°C / min, reacting at the reaction temperature for 10-90min to obtain a fifth solid product; wherein the reaction temperature is 60-90°C, and the content of alkali in the third solution containing alkali is 0.45-2mol / L; S5, subjecting the fifth solid product to a second ammonium exchange to obtain a sixth solid product; S6, mixing the sixth solid product with a fourth solution containing a phosphorus source, and subjecting the obtained second slurry to a third drying and a fifth roasting.
[0086] According to the present disclosure, the total amount of the second template, the third solvent and the fourth solvent, the molar ratio of the second alkali metal hydroxide and the second inorganic silicon source can vary in a wide range, for example, it can be (0.06-0.55): (10-100): (0.02-1.5): 1, preferably (0.08-0.50): (15-85): (0.03-1.2): 1, and the molar ratio of the second inorganic silicon source to the second aluminum source can be (20-500): 1; wherein the second inorganic silicon source is calculated as SiO2, the second alkali metal hydroxide is calculated as alkali metal oxide (for example, when the second alkali metal hydroxide is NaOH, the second alkali metal hydroxide is calculated as Na2O), and the second aluminum source is calculated as Al2O3. In one embodiment, the second template and the second alkali metal hydroxide contain OH - The ratio of the total molar amount of to the molar amount of the second inorganic silicon source calculated as SiO2 (abbreviated as OH / SiO2) is (0.01-1.5):1, preferably (0.02-1.2):1.
[0087] According to the present disclosure, hydrothermal treatment is well known to those skilled in the art, and can be performed in a heat-resistant sealed container, for example. The present disclosure does not limit the pressure of the hydrothermal treatment, and the hydrothermal treatment can be performed under the autogenous pressure of the reaction system or under an applied pressure, preferably under autogenous pressure.
[0088] According to the present disclosure, in step S2, the molar ratio of the second alkali metal hydroxide calculated as alkali metal oxide, the fourth solvent and the second aluminum source calculated as Al2O3 is preferably (2.0-4.5): (80-350): 1.
[0089] In one embodiment, the conditions of the third hydrothermal treatment include: a temperature of 160-180° C. and a time of 12-60 hours.
[0090] According to the present disclosure, in step S4, the weight ratio of the fourth solid product to the third alkali-containing solution can be 1:(2-10), and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the fourth solid product is 1.2-5.0.
[0091] According to the present disclosure, in step S5, the second ammonium exchange of the fifth solid product comprises: mixing the fifth solid product, the second ammonium source and the sixth solvent in a weight ratio of 1: (0.5-2): (5-20), and reacting the obtained mixture at 50-100°C, preferably 60-90°C for 0.5-2 hours. The second ammonium source is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate. The ammonium exchange can be performed once or multiple times. Optionally, the product obtained by the second ammonium exchange is filtered, washed and dried; optionally, the product obtained by the second ammonium exchange is subjected to the seventh roasting, preferably, the product obtained by the second ammonium exchange is subjected to the seventh roasting after filtering, washing and drying; the temperature of the seventh roasting can be 400-600°C, and the time can be 1-24 hours, preferably 1-10 hours or 1.5-6 hours, more preferably, the temperature is 450-580°C, and the time is 2-4.5 hours.
[0092] According to the present disclosure, in step S6, the weight ratio of the fourth solution containing the phosphorus source to the sixth solid product can be 1:(0.5-2.0). The mass content of the phosphorus source in the fourth solution is, for example, 1-10%.
[0093] According to the present disclosure, compared with the fourth solid product, the mesopore specific surface area of the hollow ZSM-5 multi-level pore molecular sieve (sixth solid product) increases by 100-500%, the mesopore volume increases by 150-600%, and the total acid content increases by 50-250%.
[0094] According to the present disclosure, roasting is a technical means conventionally adopted by those skilled in the art, and the roasting can be performed in a muffle furnace, a tube furnace, etc. The conditions of the second roasting, the third roasting, the fourth roasting, and the fifth roasting each independently include: a temperature of 400-600° C. and a time of 2-6 hours, preferably, a temperature of 450-580° C. and a time of 2.5-4.5 hours.
[0095] According to the present disclosure, drying is a technical means commonly used by those skilled in the art, and roasting can be performed in a constant temperature drying oven. The conditions of the second drying and the third drying each independently include: a temperature of 90-120° C. and a time of 2-24 hours.
[0096] According to the present disclosure, the first organic silicon source is selected from one or more of methyl orthosilicate and ethyl orthosilicate; the second inorganic silicon source is selected from one or more of silica sol, water glass and solid silica gel; the first template and the second template are each independently selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, n-butylamine and hexamethylenediamine; the first aluminum source and the second aluminum source are each independently selected from one or more of sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol; the first alkali metal hydroxide and the second alkali metal hydroxide are each independently selected from one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide; the first alkali solution and the second alkali solution are each independently selected from one or more of sodium hydroxide solution, potassium hydroxide solution, lithium hydroxide and barium hydroxide; the phosphorus source is selected from at least one or more of phosphoric acid, diammonium phosphate, diammonium hydrogen phosphate and ammonium phosphate.
[0097] In a specific embodiment of the present disclosure, the method further comprises: mixing the catalyst particles obtained by the first drying and the optional first calcination, the ammonium salt and the fifth solvent in a weight ratio of 1: (0.1-1): (5-15) and then performing a third ammonium exchange, and optionally washing; the conditions of the third ammonium exchange include: a temperature of 50-100° C. and a time of 0.5-2 hours; the solution containing the ammonium salt is calculated as an ammonium salt, and the ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate. The ammonium exchange can be performed multiple times.
[0098] According to the present disclosure, in one embodiment, the first solvent, the second solvent, the third solvent, the fourth solvent, the fifth solvent and the sixth solvent are each water.
[0099] The third aspect of the present disclosure provides an application of the composite catalyst provided in the first aspect of the present disclosure in increasing the production of light olefins in hydrogenation LCO catalytic cracking or heavy oil catalytic cracking. Wherein, when the second molecular sieve is a molecular sieve with a pore size of 0.56-0.75 nm, the composite catalyst is used in hydrogenation LCO catalytic cracking to increase the production of light olefins; when the second molecular sieve is a rare earth-containing Y-type molecular sieve, the composite catalyst is used in heavy oil catalytic cracking to increase the production of light olefins.
[0100] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0101] The raw materials used in the following examples and comparative examples are commercially available unless otherwise specified, wherein kaolin is an industrial product of China Kaolin Corporation, with a solid content of 75% by weight; pseudo-boehmite is produced by Shandong Aluminum Plant, with an alumina content of 65% by weight; aluminum sol is produced by Qilu Branch of Sinopec Catalyst Co., Ltd., with an alumina content of 21% by weight; silica sol is produced by Beijing Chemical Plant, with a silicon oxide content of 25% by weight (acidic silica sol, pH 3.0); concentrated hydrochloric acid is chemically pure, produced by Beijing Chemical Plant. β molecular sieve, brand BETA-25-NKC, pore size of 0.59 nm, produced by Tianjin Nanhua Catalyst Co., Ltd., its SEM picture is as follows Figure 3 Y-type molecular sieve, grade SCY-12, rare earth content 12% by weight, produced by Qilu Branch of Sinopec Catalyst Co., Ltd., its SEM picture is as shown in Figure 4 shown.
[0102] In the embodiments and comparative examples, the crystal size of the molecular sieve was measured by SEM, and 10 crystal sizes were randomly measured and the average value was taken to obtain the average crystal size of the molecular sieve sample.
[0103] The bulk silicon-aluminum ratio of the sample was determined by XRF method, the instrument was ZSX Primus II (Rigaku) X-ray fluorescence spectrometer; the test conditions were: excitation voltage 50kV, excitation current 50mA, rhodium and palladium. The intensity of each element peak was measured by scintillation counter and proportional counter to analyze the elemental composition of the molecular sieve.
[0104] The surface silicon-aluminum molar ratio of the sample was determined by the XPS method, using the ESCALab250 X-ray photoelectron spectrometer from ThermoFisher, under the following test conditions: the excitation source was monochromatic Al Kα X-ray, the excitation energy was 1496.6 eV, and the power was 150 W. The electron binding energy was corrected using the C1s peak (284.8 eV) of the contaminated carbon.
[0105] The total specific surface area, mesopore specific surface area and N2 adsorption-desorption curve of the sample were detected by BET adsorption full analysis method. Instrument: ASAP 2420 adsorption instrument from Micromeritics, USA. Test conditions: The sample was vacuum degassed at 100℃ and 300℃ for 0.5h and 6h respectively, and N2 adsorption-desorption test was carried out at 77.4K. The adsorption and desorption amount of nitrogen of the purified sample under different specific pressure conditions were tested to obtain the N2 adsorption-desorption isotherm. The BET specific surface area was calculated by BET formula, the micropore area was calculated by t-plot, and the pore size distribution was calculated by BJH.
[0106] The relative crystallinity of the sample was detected by X-ray diffraction method, instrument: Empyrean. Test conditions: tube voltage 40 kV, tube current 40 mA, Cu target Kα radiation, 2θ scanning range 5°-35°, scanning rate 2 (°) / min.
[0107] The phosphorus-aluminum molar ratio of the sample is detected by X-ray fluorescence method. Instrument: ZSX Primus II (Rigaku) X-ray fluorescence spectrometer. Test conditions: excitation voltage 50kV, excitation current 50mA, rhodium-palladium. The intensity of each element peak is measured by scintillation counter and proportional counter to analyze the elemental composition of molecular sieve.
[0108] The strong B acid content and total B acid content of the sample were detected by pyridine infrared adsorption method, and the strong L acid content and total L acid content were detected by pyridine infrared adsorption method. Instrument: NICOLET 6700 Fourier transform infrared spectrometer of BIQ-RAD Company, USA. Test method: After the sample is pressed into a tablet, it is placed in the in-situ cell of the infrared spectrometer and sealed, and adsorption and desorption are carried out according to the set program. The pyridine adsorbed acid content is calculated by peak area.
[0109] Examples 1-3 are examples of preparing phosphorus-containing hollow ZSM-5 multi-level pore molecular sieves
[0110] Example 1
[0111] (1) 456.0 g of ethyl orthosilicate was weighed, and 3115.7 g of deionized water was added. The mixture was stirred and heated in a water bath at 40° C. for 2 h, and then the water bath temperature was raised to 70° C. and stirred and heated for 4 h to remove ethanol produced by hydrolysis of the silicon source. During this process, water evaporated simultaneously with the ethanol was intermittently added to the system. The obtained mixed liquid was mixed and stirred with 558.3 g of a tetrapropylammonium hydroxide aqueous solution (mass fraction of 25.0%) at 25° C. for 1 h to obtain a first mixed product;
[0112] (2) weighing 17.2 g of sodium hydroxide particles, adding 384.0 g of deionized water to completely dissolve the sodium hydroxide, then adding 40.8 g of aluminum nitrate nonahydrate, and stirring at room temperature for 1.0 h to obtain a second mixed product (i.e., an aluminum source solution);
[0113] (3) slowly adding the second mixed product to the first mixed product, mixing evenly, stirring at room temperature for 4.0 hours, transferring the obtained precursor solution into a synthesis reactor, and dynamically crystallizing at 170° C. for 48 hours; after the crystallization, centrifugally filtering, washing, drying, and calcining at 550° C. for 4 hours to obtain the first solid product (referred to as molecular sieve I-M1);
[0114] (4) mixing the first solid product and a sodium hydroxide solution with a concentration of 0.5 mol / L, wherein the mass ratio of the first solid product to the alkaline solution is 1:10, heating the temperature to 80°C at a heating rate of 2°C / min, stirring at the temperature for 30 min, filtering, washing, and drying to obtain a second solid product (referred to as molecular sieve I-S1-Na);
[0115] (5) The second solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:1:10, stirred and heated in a water bath at 80°C for 30 min, filtered, washed, and dried; the obtained solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:0.5:10, subjected to a second ammonium exchange, filtered, washed, dried, and calcined at 550°C for 2 h to obtain a third solid product (a hydrogen-type hollow ZSM-5 multi-level pore molecular sieve, denoted as I-S1-H).
[0116] (6) 2.69 g of H3PO4 solution (concentration of 85 wt%) was dissolved in 46.25 g of deionized water, and the solution was stirred evenly to obtain a phosphorus-containing solution; 50 g of the third solid product was spread evenly on a surface dish, and the phosphorus-containing solution was slowly added dropwise, and the mixture was mixed evenly to make the molecular sieve present a "viscous paste", and the mixture was dried at 115° C. in an air atmosphere for 4 h, and then calcined at 550° C. for 2 h to obtain a phosphorus-containing hollow ZSM-5 hierarchical pore molecular sieve, which was designated as SS-1. Its SEM photograph is shown in FIG. Figure 1 The properties of the samples are shown in Table 1.
[0117] Example 2
[0118] (1) weighing 550.0 g of methyl orthosilicate, adding 2975.0 g of deionized water, stirring and heating in a water bath at 30° C. for 5 h, raising the water bath temperature to 70° C. and stirring for 4 h to remove ethanol produced by hydrolysis of the silicon source, intermittently replenishing the system with water evaporated simultaneously with the ethanol during the process, and mixing the obtained mixed liquid with 241.5 g of a tetrapropylammonium bromide aqueous solution (mass fraction of 25.0%) at 20° C. and stirring for 0.5 h to obtain a first mixed product;
[0119] (2) weighing 9.1 g of sodium hydroxide particles, adding 217.0 g of deionized water to completely dissolve the sodium hydroxide, then adding 6.0 g of sodium aluminate (alumina content is 62.0%), stirring at 20° C. for 2.0 h, and obtaining a second mixed product;
[0120] (3) slowly adding the second mixed product to the first mixed product, mixing evenly, and stirring at room temperature for 4.0 hours; transferring the obtained precursor solution into a synthesis reactor, and dynamically crystallizing at 180° C. for 24 hours; after the crystallization, centrifugally filtering, washing, drying, and calcining at 550° C. for 4 hours to obtain the first solid product (referred to as molecular sieve I-M2);
[0121] (4) mixing the first solid product and a sodium hydroxide alkaline solution having a concentration of 0.6 mol / L, wherein the mass ratio of the first solid product to the alkaline solution is 1:10, heating the mixture to 80°C at a heating rate of 4°C / min, and then heating and stirring the mixture at 80°C for 30 min, filtering, washing, and drying to obtain a second solid product (referred to as molecular sieve I-S2-Na);
[0122] (5) The second solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:1:10, stirred and heated in a water bath at 80°C for 30 min, filtered, washed, and dried, and the obtained solid product: ammonium chloride: deionized water = 1:0.5:10 is mixed uniformly, subjected to a second ammonium exchange, filtered, washed, dried, and calcined at 550°C for 2 h to obtain a third solid product (hydrogen-type hollow ZSM-5 multi-level pore molecular sieve, denoted as I-S2-H).
[0123] (6) Dissolve 2.68 g of ammonium dihydrogen phosphate in 44.21 g of deionized water, fully dissolve, and stir to obtain a phosphorus-containing solution; spread 50 g of the third solid product on a surface dish, slowly drop the prepared phosphorus-containing solution, and fully mix to make the molecular sieve appear "viscous paste"; dry at 110° C. in air atmosphere for 4 h, and calcine at 550° C. for 2 h to obtain a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, denoted as SS-2, whose SEM photograph is shown as follows: Figure 2 The properties of the samples are shown in Table 1.
[0124] Example 3
[0125] (1) Weigh 455.9 g of tetrapropylammonium hydroxide aqueous solution (mass fraction 25.0%), add 3238.3 g of deionized water, stir at room temperature for 10 min, then add 1156.4 g of silica sol (SiO2 content 25%), stir for 1.0 h in a 50° C. water bath, transfer the obtained third mixed product into a reactor, crystallize at 80° C. for 2 h, and then heat to 170° C. for crystallization for 12 h to obtain a fourth mixed product;
[0126] (2) weighing 9.7 g of sodium hydroxide particles, adding 277.9 g of deionized water to completely dissolve the sodium hydroxide, then adding 33.3 g of aluminum nitrate nonahydrate, and stirring at 25° C. for 1.0 h to obtain a fifth mixed product;
[0127] (3) adding the fourth mixed product to the fifth mixed product, stirring evenly, and continuing to crystallize at 170° C. for 36 hours; after the crystallization is completed, centrifugation is performed, washed, dried, and calcined at 550° C. for 4 hours to obtain a fourth solid product (referred to as molecular sieve I-M3);
[0128] (4) mixing the fourth solid product and a sodium hydroxide solution with a concentration of 1.0 mol / L, wherein the mass ratio of the fourth solid product to the alkaline solution is 1:10, heating the temperature to 80°C at a heating rate of 5°C / min, stirring at the temperature for 30 min, filtering, washing, and drying to obtain a fifth solid product (referred to as molecular sieve I-S3-Na);
[0129] (5) The fifth solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:1:10, stirred and heated in a water bath at 80°C for 30 min, filtered, washed, and dried, and then the obtained solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:0.5:10, subjected to a second ammonium exchange, filtered, washed, dried, and calcined at 550°C for 2 h to obtain a sixth solid product (referred to as I-S3-H).
[0130] (6) Dissolve 1.71 g of H3PO4 solution (concentration 85 wt%) in 42.49 g of deionized water, stir evenly to fully dissolve, and obtain a phosphorus-containing solution; spread 50 g of the sixth solid product on a surface dish, slowly drop the prepared phosphorus-containing solution, and mix evenly to make the molecular sieve appear "viscous paste"; dry at 115°C in an air atmosphere for 4 h, and then calcine at 550°C for 2 h to obtain a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, denoted as SS-3, and its properties are listed in Table 1.
[0131] Comparative Example 1
[0132] Conventional crystalline ZSM-5 molecular sieve DSS-1 was purchased from Qilu Branch of Sinopec Catalyst Company, with a silicon-aluminum molar ratio (SiO2 / Al2O3) of 25. Its properties are listed in Table 1.
[0133] Table 1
[0134]
[0135]
[0136] In Table 1, R represents a template, and the bulk-surface silicon-aluminum molar ratio represents the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio;
[0137] Increased value of mesoporous specific surface area = 100% × [mesoporous specific surface area of hollow ZSM-5 multi-level pore molecular sieve (or hollow multi-level pore ZSM-5 nanocrystalline material, hydrogen-type hollow ZSM-5 multi-level pore molecular sieve before introduction of phosphorus) / mesoporous specific surface area of the first solid product (or fourth solid product) - 1];
[0138] Mesopore specific volume increase value = 100% × [mesopore specific volume of hollow ZSM-5 hierarchical pore molecular sieve (or hollow multi-level pore ZSM-5 nanocrystalline material, hydrogen-type hollow ZSM-5 hierarchical pore molecular sieve before introduction of phosphorus) / mesopore specific volume of the first solid product (or fourth solid product) - 1];
[0139] Total acid increase value = 100% × [total acid amount of hollow ZSM-5 multi-level pore molecular sieve (or hollow multi-level pore ZSM-5 nanocrystalline material, hydrogen-type hollow ZSM-5 multi-level pore molecular sieve before the introduction of phosphorus) / total acid amount of the first solid product (or the fourth solid product) - 1].
[0140] Examples 4-9 and Comparative Examples 2-5 are examples of preparing composite catalysts
[0141] Embodiment 4-6
[0142] Catalysts were prepared using the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieves prepared in Examples 1-3, and the catalyst numbers were A1-A3.
[0143] The preparation method of the composite catalyst comprises:
[0144] (1) Pseudo-boehmite and water are uniformly mixed, and concentrated hydrochloric acid with a concentration of 36% by weight is added under stirring, and the acid-aluminum molar ratio is 0.2 (the weight ratio of HCl to pseudo-boehmite calculated as Al2O3); the resulting mixture is aged at 70°C for 1.5 hours to obtain an aged pseudo-boehmite slurry. The aged pseudo-boehmite slurry has an aluminum oxide content of 12% by weight;
[0145] (2) mixing the prepared phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, β molecular sieve, aluminum sol, silica sol, kaolin, the aged pseudo-boehmite slurry and deionized water to form a slurry with a solid content of 30% by weight, and spray drying to obtain catalyst microspheres;
[0146] (3) calcining the catalyst microspheres at 550°C for 4 h;
[0147] (4) The calcined catalyst microspheres were exchanged at 80°C for 1 hour according to a weight ratio of catalyst microspheres: ammonium salt: H2O = 1:1:10, filtered, and the above exchange and filtration process was repeated once, and dried, wherein the ammonium salt was ammonium chloride, and the sodium oxide content in the obtained composite catalyst was less than 0.15% by weight. The composition of the prepared catalyst is shown in Table 2.
[0148] Comparative Example 2
[0149] Catalyst DA1 was prepared by the method of Example 4, except that molecular sieve DSS-1 of Comparative Example 1 was used instead of molecular sieve SS-1 prepared in Example 1. The composition of the prepared catalyst is shown in Table 2.
[0150] Comparative Example 3
[0151] Catalyst DA2 was prepared by the same method as in Example 4, except that the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve was not added. The composition of the prepared catalyst is shown in Table 2.
[0152] Embodiment 7-9
[0153] According to the method of Example 4, the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieves prepared in Examples 1-3 were used to prepare catalysts, except that the second molecular sieves in Examples 7-9 were Y-type molecular sieves (SCY-12 molecular sieves), and the catalyst numbers were A4-A6. The compositions of the prepared catalysts are shown in Table 2.
[0154] Comparative Example 4
[0155] Catalyst DA3 was prepared by the method of Example 7, except that the molecular sieve DSS-1 of Comparative Example 1 was used instead of the molecular sieve SS-1 prepared in Example 1. The composition of the prepared catalyst is shown in Table 2.
[0156] Comparative Example 5
[0157] Catalyst DA4 was prepared by the same method as in Example 7, except that phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve was not added. The composition of the prepared catalyst is shown in Table 2.
[0158] Table 2
[0159]
[0160] Test Example 1
[0161] After the composite catalysts prepared in Examples 4-6 and Comparative Examples 2-3 were aged at 820°C and 100% by volume steam for 30 hours, their hydrogenation LCO catalytic cracking performance was evaluated in a small fixed fluidized bed reactor. The evaluation conditions were a reaction temperature of 620°C and a weight space velocity of 4 h -1 , catalyst-oil weight ratio 12. The properties of hydrogenated LCO are shown in Table 3, and the reaction results are shown in Table 4. The product mass distribution is calculated based on the raw material feed.
[0162] Table 3
[0163]
[0164]
[0165] Table 4
[0166] Example 4 Example 5 Example 6 Comparative Example 2 Comparative Example 3 catalyst A1 A2 A3 DA1 DA2 Dry gas, weight % 14.37 14.34 13.02 6.81 2.54 Liquefied gas, weight % 38.64 37.46 36.53 20.13 8.59 Gasoline, weight % 26.30 26.80 27.91 38.49 15.63 Diesel, weight % 12.05 13.41 14.73 23.01 37.50 Heavy oil, weight % 1.67 1.97 2.67 7.80 34.87 Coke, weight % 6.97 6.02 5.14 3.76 0.87 Light olefins, weight % 39.79 39.22 37.47 19.9 6.11 Ethylene, weight % 9.64 9.13 8.97 4.38 1.01 Propylene, weight % 19.46 19.67 18.63 10.05 2.67 Butene, weight % 10.69 10.42 9.87 5.47 2.43
[0167] It can be seen from Table 4 that the composite catalyst provided by the present disclosure has better hydrogenation LCO catalytic cracking ability and higher light olefin yield.
[0168] Test Example 2
[0169] After aging the composite catalysts prepared in Examples 7-9 and Comparative Examples 4-5 for 30 hours at 820°C and 100% by volume water vapor, their heavy oil catalytic cracking reaction performance was evaluated in a small fixed fluidized bed reactor, and the evaluation conditions were a reaction temperature of 520°C and a catalyst-to-oil weight ratio of 10. The properties of the heavy oil are shown in Table 5, and the reaction results are shown in Table 6. The product mass distribution is calculated based on the raw material feed.
[0170] Table 5
[0171]
[0172]
[0173] Table 6
[0174] Example 7 Example 8 Example 9 Comparative Example 4 Comparative Example 5 catalyst A4 A5 A6 DA3 DA4 Dry gas, weight % 8.6 8.4 8.27 5.18 3.69 Liquefied gas, weight % 38.47 37.67 36.49 33 28.42 Gasoline, weight % 36.52 36.84 35.53 33.67 42.62 Diesel, weight % 7.75 7.18 6.87 16.07 14.28 Heavy oil, weight % 3.58 4.05 5.97 8.02 7.11 Coke, weight % 5.08 5.86 6.87 4.06 3.88 Ethylene, weight % 4.01 3.84 3.65 3.08 2.27 Propylene, weight % 16.54 15.14 14.06 10.57 4.59 C4 olefins, weight % 10.02 9.04 8.76 6.25 3.42
[0175] It can be seen from Table 6 that the composite catalyst provided by the present disclosure has better heavy oil conversion ability and higher light olefin yield.
[0176] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0177] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0178] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A composite catalyst, characterized in that: The composite catalyst contains a phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve, a second molecular sieve and a carrier. Based on the dry weight of the composite catalyst, the content of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 5-35% by weight, the content of the second molecular sieve is 10-50% by weight, and the content of the carrier is 30-80% by weight. The phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve has a hollow structure, an average grain size of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, a ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the total specific surface area of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 340-400 m 2 / g, mesoporous specific surface area is 40-150m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area; the strong B acid content of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve accounts for 65-80% of the total B acid content, and the strong L acid content accounts for 50-75% of the total L acid content; The second molecular sieve is a molecular sieve with a pore size of 0.56-0.75 nm, or the second molecular sieve is a Y-type molecular sieve containing rare earth.
2. The composite catalyst according to claim 1, wherein The phosphorus-aluminum molar ratio of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 0.2-1.
3.
3. The composite catalyst according to claim 1, wherein The average grain size of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve grains is 0.4-2.5 μm, the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.1-1.4, and the relative crystallinity is 75-90%.
4. The composite catalyst according to claim 1, wherein The total specific surface area of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve is 350-400m 2 / g, mesopore specific surface area is 45-140m 2 / g, and the mesoporous specific surface area accounts for 20-35% of the total specific surface area.
5. The composite catalyst according to claim 1, wherein The molecular sieve with a pore size of 0.56-0.75 nm is one or more of the molecular sieves having AET, AFR, AFS, AFI, BEA, BOG, CFI, CON, GME, IFR, ISV, LTL, MEI, MOR, OFF and SAO structures; preferably at least one of Beta, SAPO-5, SAPO-40, SSZ-13, CIT-1, ITQ-7, ZSM-18, mordenite and gmelinite; The rare earth content of the Y-type molecular sieve is 2-25% by weight as rare earth element oxide, and the rare earth element is lanthanum and / or cerium; the phosphorus content of the Y-type molecular sieve is 0-10% by weight as P2O5; the Y-type molecular sieve is selected from one or more of REY molecular sieve, DASY molecular sieve, USY molecular sieve, phosphorus-containing DASY molecular sieve, phosphorus-containing USY molecular sieve, PSRY molecular sieve, HRY molecular sieve, HSY molecular sieve, SCY molecular sieve, and RSCY molecular sieve.
6. The composite catalyst according to claim 1, wherein The carrier is selected from one or more of natural clay, alumina carrier, silica carrier, aluminum phosphate carrier and silica-alumina carrier; Preferably, the silica carrier is one or more of neutral silica sol, acidic silica sol or alkaline silica sol; the alumina carrier is one or more of aluminum sol, acidified pseudo-boehmite, hydrated alumina and activated alumina; the aluminum phosphate carrier is phosphate aluminum gel; the silica aluminum oxide carrier is one or more of solid silica aluminum material, silica aluminum sol and silica aluminum gel.
7. The composite catalyst according to claim 1, wherein The carrier comprises a silicon oxide carrier; based on the dry weight of the composite catalyst, the content of the silicon oxide carrier in terms of SiO2 is 1-20% by weight.
8. A method for preparing the composite catalyst according to any one of claims 1 to 7, the method comprising: The slurry containing the support, the phosphorus-containing hollow ZSM-5 hierarchical pore molecular sieve, the second molecular sieve and water is subjected to a first drying and an optional first calcination.
9. The method according to claim 8, wherein: The preparation steps of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve include: (1) Mixing a first organosilicon source and a first solvent at 30-50° C. and stirring for 0.5-5 hours, then heating to 70-100° C. and stirring for 2-10 hours, and mixing the obtained mixed liquid with a first template at 20-30° C. for 0.5-3.0 hours to obtain a first mixed product; (2) mixing a first alkali metal hydroxide, a second solvent and a first aluminum source, calculated as Al2O3, in a molar ratio of (1.5-5):(60-350):1 at 20-80° C. for 0.5-2.0 hours to obtain a second mixed product; (3) mixing the first mixed product and the second mixed product and subjecting them to dynamic crystallization, taking out the obtained solid and subjecting it to a second calcination to obtain a first solid product; (4) mixing the first solid product with a first solution containing alkali, heating the mixture to a reaction temperature at a heating rate of 1-5° C. / min, and reacting the mixture at the reaction temperature for 10-90 min to obtain a second solid product; wherein the reaction temperature is 60-90° C., and the content of alkali in the first solution containing alkali is 0.45-2 mol / L; (5) subjecting the second solid product to a first ammonium exchange, and optionally a sixth calcination, to obtain a third solid product; (6) mixing the third solid product with a second solution containing a phosphorus source, and subjecting the obtained first slurry to a second drying and a third calcination; or, The preparation steps of the phosphorus-containing hollow ZSM-5 multi-level pore molecular sieve include: S1, mixing the second template, the second inorganic silicon source and the third solvent at 30-50° C. for 0.5-3.0 hours, and subjecting the obtained third mixed product to a first hydrothermal treatment and a second hydrothermal treatment in sequence to obtain a fourth mixed product; wherein the conditions of the first hydrothermal treatment include: a temperature of 80-150° C. and a time of 1-6 hours; the conditions of the second hydrothermal treatment include: a temperature of 160-180° C. and a time of 4-60 hours; S2, mixing a second alkali metal hydroxide, calculated as alkali metal oxide, a fourth solvent, and a second aluminum source, calculated as Al2O3, at a molar ratio of (1.5-5):(60-350):1 at 20-80° C. for 0.5-2.0 hours to obtain a fifth mixed product; S3, mixing the fourth mixed product and the fifth mixed product, subjecting the obtained mixture to a third hydrothermal treatment, taking out the obtained solid and subjecting it to a fourth roasting to obtain a fourth solid product; S4, mixing the fourth solid product with the third solution containing alkali, raising the temperature to the reaction temperature at a heating rate of 1-5°C / min, and reacting at the reaction temperature for 10-90min to obtain a fifth solid product; wherein the reaction temperature is 60-90°C, and the content of alkali in the third solution containing alkali is 0.45-2mol / L; S5, subjecting the fifth solid product to a second ammonium exchange, and optionally a seventh roasting, to obtain a sixth solid product; S6. Mixing the sixth solid product with the fourth solution containing a phosphorus source, and subjecting the obtained second slurry to a third drying and a fifth calcination.
10. The method according to claim 9, wherein: The first organic silicon source is selected from one or more of methyl orthosilicate and ethyl orthosilicate; The second inorganic silicon source is selected from one or more of silica sol, water glass and solid silica gel; The first template agent and the second template agent are each independently selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, n-butylamine and hexamethylenediamine; The first aluminum source and the second aluminum source are each independently selected from one or more of sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol; The first alkali metal hydroxide and the second alkali metal hydroxide are each independently selected from one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide; The first alkali-containing solution and the third alkali-containing solution are each independently selected from one or more of a sodium hydroxide solution, a potassium hydroxide solution, a lithium hydroxide solution and a barium hydroxide solution; The phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate.
11. The method according to claim 9, wherein: The molar ratio of the total amount of the first template, the first solvent and the second solvent, the first alkali metal hydroxide, and the first organic silicon source is (0.06-0.55): (10-100): (0.02-1.5): 1; the molar ratio of the first organic silicon source to the first aluminum source is (20-500): 1; wherein the first organic silicon source is calculated as SiO2, the first alkali metal hydroxide is calculated as alkali metal oxide, and the first aluminum source is calculated as Al2O3; Preferably, in step (2), the molar ratio of the first alkali metal hydroxide, calculated as alkali metal oxide, the second solvent and the first aluminum source, calculated as Al2O3, is (2-4.5): (80-350): 1; Preferably, in step (4), the molar ratio of the first solid product to the first alkali-containing solution is 1:(2-10), the first solid product is calculated as SiO2, and the first alkali-containing solution is calculated as alkali metal oxide; the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the first solid product is 1.2-5.0; Preferably, in step (6), the weight ratio of the second solution containing the phosphorus source to the third solid product is 1:(0.5-2.0); The molar ratio of the total amount of the second template, the third solvent and the fourth solvent, the amount of the second alkali metal hydroxide and the second inorganic silicon source is (0.06-0.55): (10-100): (0.02-1.5): 1, and the molar ratio of the second inorganic silicon source to the second aluminum source is (20-500): 1; wherein the second inorganic silicon source is calculated as SiO2, the second alkali metal hydroxide is calculated as alkali metal oxide, and the second aluminum source is calculated as Al2O3; Preferably, in step S2, the molar ratio of the second alkali metal hydroxide, the fourth solvent and the second aluminum source, calculated as Al2O3, is (2-4.5): (80-350): 1; Preferably, in step S4, the molar ratio of the fourth solid product to the third alkali-containing solution is 1:(2-10), the fourth solid product is calculated as SiO2, the third alkali-containing solution is calculated as alkali metal oxide, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the fourth solid product is 1.2-5.0; Preferably, in step S6, the weight ratio of the fourth solution containing the phosphorus source to the sixth solid product is 1:(0.5-2.0).
12. The method according to claim 9, wherein: The conditions of the dynamic crystallization include: a temperature of 160-180° C. and a time of 12-60 hours; The conditions of the third hydrothermal treatment include: temperature of 160-180°C and time of 12-60 hours; The conditions of the second calcination, the third calcination, the fourth calcination and the fifth calcination are independently as follows: a temperature of 400-600° C. and a time of 2-6 hours; The conditions of the second drying and the third drying each independently include: a temperature of 90-120° C. and a time of 2-24 hours.
13. The method according to claim 8, wherein: The method further comprises: mixing the catalyst particles obtained by the first drying and the optional first calcination, the ammonium salt and the fifth solvent in a weight ratio of 1:(0.1-1):(5-15) to perform a third ammonium exchange, and optionally washing; The conditions of the third ammonium exchange include: temperature of 50-100° C. and time of 0.5-2 hours; The ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate.
14. Use of the composite catalyst according to any one of claims 1 to 7 in increasing the production of light olefins in hydrogenation LCO catalytic cracking or heavy oil catalytic cracking.
Citation Information
Patent Citations
Catalytic cracking catalyst
CN114749208A
Petroleum hydrocarbon catalytic cracking catalyst
CN114797962A
Process for producing light olefins by using a ZSM - 5 - based catalyst
WO2012059191A1