Modified titanium silicalite molecular sieve, titanium silicalite molecular sieve supported gold nanoparticle catalyst, preparation method of modified titanium silicalite molecular sieve supported gold nanoparticle catalyst and propylene gas-phase epoxidation method

By modifying the titanium-silicon molecular sieve, a weakly acidic carrier is formed to load 0-valent Au nanoparticles, which solves the problem of the impact of carrier performance on the valence state of Au nanoparticles and improves the conversion rate and selectivity of propylene gas-phase epoxidation reaction.

CN118767987APending Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310376039.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, there are few studies on the effect of carrier performance on the valence state and quantity of Au nanoparticles, which results in unstable catalytic activity of Au nanoparticles in titanium-silicon molecular sieve catalysts and affects the selectivity and conversion rate of propylene gas phase epoxidation reaction. .

Method used

By modifying the titanium-silicon molecular sieve, reducing its acidity, forming a weakly acidic carrier, and loading gold nanoparticles to maintain the 0-valent state, the propylene conversion rate and propylene oxide selectivity of the catalyst can be improved. The modification process includes using nitrate to modify the titanium-silicon molecular sieve, and adjusting the acid amount and acidic distribution through the NH3-TPD spectrum to ensure that the total acid amount is within the range of 0.2-0.5mmol/g, and the molar ratio of titanium to silicon is within 0.001-0.04:1, the loaded Au element accounts for more than 90% of the 0-valent Au.

Benefits of technology

It significantly improves the propylene conversion rate of propylene gas phase epoxidation reaction to 8-16%, maintains high propylene oxide selectivity of 85-95%, and improves the stability of the catalyst and reaction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767987A_ABST
    Figure CN118767987A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic chemistry and catalytic chemistry, and discloses a modified titanium silicalite molecular sieve, a titanium silicalite molecular sieve supported gold nanoparticle catalyst, a preparation method and a propylene gas-phase epoxidation method. The peak position of the NH3-TPD spectrogram of the modified titanium silicalite molecular sieve is 50-200 DEG C, and the total acid content detected and calculated by NH3-TPD is 0.2-0.5 mmol / g. The catalyst comprises a carrier and gold nanoparticles loaded on the carrier, the proportion of zero-valent Au in the gold nanoparticles is larger than 90% in terms of Au element, and the zero-valent Au in the gold nanoparticles is obtained through XPS detection and calculation. The modified titanium silicalite molecular sieve provided by the invention is relatively weak in acidity and relatively low in acid content, is beneficial to keeping zero valence of gold nanoparticles loaded on the modified titanium silicalite molecular sieve, and can obtain relatively high propylene conversion rate and epoxypropane selectivity when being applied to propylene gas-phase epoxidation reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic chemistry and catalytic chemistry, and in particular to a modified titanium silicate molecular sieve and a titanium silicate molecular sieve loaded with gold nanoparticle catalyst and a preparation method thereof, and a method for gas-phase epoxidation of propylene. Background Art

[0002] Bifunctional catalysts have two catalytic active centers, can catalyze two types of reactions at the same time, and have two functions, such as metal function and acid function at the same time. Molecular sieve-loaded metal nanoparticle catalysts are typical bifunctional catalysts, which have both the catalytic performance of metal nanoparticles and the acid catalytic performance or catalytic oxidation performance of molecular sieves. For example, titanium silicalite-loaded metal nanoparticle catalysts are used to catalyze the gas-phase epoxidation reaction of propylene. Existing studies have found catalysts with metal nanoparticles such as Pd, Pt, Ag, Au and their alloys loaded on titanium silicalite, and their effects on catalyzing the gas-phase epoxidation reaction of propylene are good. The reaction principle is that metal nanoparticles catalyze hydrogen and oxygen to synthesize hydrogen peroxide in situ, and then hydrogen peroxide combines with titanium silicalite to form catalytic oxidation sites, catalyzing propylene to produce propylene oxide. In recent years, researchers have continuously improved titanium silicalite-loaded metal nanoparticle catalysts in order to improve the selectivity of propylene oxide and the conversion rate of propylene. From the mechanism of propylene gas-phase epoxidation reaction, it can be seen that Au nanoparticles are the key active sites that promote the generation of H2O2. The study found that the Au nanoparticles deposited on the TS-1 carrier have various morphologies, and their catalytic activity is deeply affected by factors such as particle size, loading amount, loading position, and chemical state.

[0003] The Au species deposited by the deposition precipitation method (DP) usually exist in the TS-1 support in the form of ions. Therefore, the Au / TS-1 catalyst must be activated first to make the Au species present in the metallic state (Au 0 ) can play its catalytic role in the gas phase epoxidation of propylene. Using different atmospheres to activate Au / TS-1 catalyst will result in different Au valence states. Studies have shown that the activation atmosphere of H2 and reaction gas (H2+O2+C3H6+N2) will promote the Au 1+ Species conversion to Au 0 , while O2 atmosphere does not change Au 1+ state. Au in H2 atmosphere 1+ Disproportionate to catalytically active Au 0 , and the Cl remaining on the catalyst surface - The catalytic performance was significantly improved by removing the Au nanoparticles in the Au / TS-1 catalyst in the form of HCl. In addition to reducing the Au nanoparticles in the Au / TS-1 catalyst to a zero-valent catalytic state through activation, the properties of the carrier also have an effect on the charge state of the Au nanoparticles, but there are few studies on this aspect. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem that there is little research on the influence of carrier performance on the valence state and quantity of Au nanoparticles in the prior art, and to provide a modified titanium silicalite and a titanium silicalite-loaded gold nanoparticle catalyst and a preparation method and a method for gas-phase epoxidation of propylene. The modified titanium silicalite provided by the present invention has weak acidity and low acid content, which is conducive to the gold nanoparticles loaded thereon to maintain zero valence, and can be applied to gas-phase epoxidation of propylene to obtain a higher propylene conversion rate and propylene oxide selectivity.

[0005] In order to achieve the above objectives, the first aspect of the present invention provides a modified titanium silicalite molecular sieve, wherein the peak position of the NH3-TPD spectrum of the modified titanium silicalite is located at 50-200°C, and the total acid content detected and calculated by NH3-TPD is 0.2-0.5mmol / g, preferably 0.2-0.4mmol / g.

[0006] Preferably, the molar ratio of titanium to silicon in the modified titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:1.

[0007] Preferably, the modified titanium silicate molecular sieve is obtained by modifying the titanium silicate molecular sieve with nitrate.

[0008] Preferably, the nitrate is selected from one or more of sodium nitrate, potassium nitrate, ammonium nitrate, calcium nitrate, magnesium nitrate, lead nitrate and cerium nitrate.

[0009] Preferably, the titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0010] Preferably, the peak position of the NH3-TPD spectrum of the titanium silicalite molecular sieve is located at 50-450°C, and the total acid amount detected and calculated by NH3-TPD is 0.5-0.95mmol / g, wherein the acid amount of weak acid is 0.015-0.15mmol / g, and the acid amount of medium-strong acid is 0.45-0.80mmol / g.

[0011] Preferably, the molar ratio of titanium to silicon in the titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:1.

[0012] The second aspect of the present invention provides a method for preparing the modified titanium silicalite described in the first aspect, the method comprising: mixing the titanium silicalite, nitrate and water, and calcining.

[0013] Preferably, the weight ratio of the titanium silicon molecular sieve, nitrate and water is 1:0.005-0.2:5-40, preferably 1:0.01-0.15:5-30.

[0014] Preferably, the titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0015] Preferably, the peak position of the NH3-TPD spectrum of the titanium silicalite molecular sieve is located at 50-450°C, and the total acid amount detected and calculated by NH3-TPD is 0.5-0.95mmol / g, wherein the acid amount of weak acid is 0.015-0.15mmol / g, and the acid amount of medium-strong acid is 0.45-0.80mmol / g.

[0016] Preferably, the molar ratio of titanium to silicon in the titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:1.

[0017] Preferably, the nitrate is selected from one or more of sodium nitrate, potassium nitrate, ammonium nitrate, calcium nitrate, magnesium nitrate, lead nitrate and cerium nitrate.

[0018] Preferably, the mixing treatment conditions include: the mixing treatment method is mixed stirring; the mixing treatment temperature is 20-80° C.; the mixing treatment time is 0.5-24 h, preferably 1-20 h.

[0019] Preferably, the calcination conditions include: a calcination temperature of 450-650° C.; and a calcination time of 4-10 h.

[0020] The third aspect of the present invention provides a modified titanium silicalite molecular sieve prepared by the method described in the second aspect.

[0021] The fourth aspect of the present invention provides a titanium silicalite loaded gold nanoparticle catalyst, the catalyst comprising a carrier and gold nanoparticles loaded on the carrier; in terms of Au element, the proportion of zero-valent Au in the gold nanoparticles is greater than 90%, as detected and calculated by XPS; the carrier is the modified titanium silicalite described in the first aspect or the modified titanium silicalite described in the third aspect.

[0022] Preferably, based on the total weight of the catalyst, the content of Au element in the catalyst is 0.01-1 wt %, preferably 0.04-0.8 wt %.

[0023] The fifth aspect of the present invention provides a method for preparing the titanium silicon molecular sieve supported gold nanoparticle catalyst according to the fourth aspect, the method comprising the following steps:

[0024] S1, mixing the modified titanium silicon molecular sieve with an aqueous solution of a gold compound, and then adjusting the pH value of the resulting mixture to alkaline;

[0025] S2, performing solid-liquid separation on the product obtained in step S1, and activating the obtained solid product;

[0026] The modified titanium silicate molecular sieve is the modified titanium silicate molecular sieve described in the first aspect or the modified titanium silicate molecular sieve described in the third aspect.

[0027] Preferably, the gold compound aqueous solution is selected from one or more of an aqueous solution of chloroauric acid, an aqueous solution of cesium chloroaurate and an aqueous solution of potassium chloroaurate.

[0028] Preferably, in step S1, the concentration of the gold compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

[0029] Preferably, in step S1, the amount of the gold-containing compound aqueous solution calculated as Au element is 0.01-5% by weight, preferably 0.1-5% by weight, of the amount of the modified titanium silicon molecular sieve.

[0030] Preferably, in step S1, the pH value of the mixture is adjusted to 7-10, preferably 7-9.

[0031] Preferably, in step S1, the pH adjuster used to adjust the pH value of the mixture is an alkaline solution.

[0032] Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

[0033] Preferably, in step S2, the activation conditions include: temperature of 150-300°C and time of 1-5 hours.

[0034] The sixth aspect of the present invention provides a titanium silicon molecular sieve loaded with gold nanoparticle catalyst prepared by the method described in the fifth aspect.

[0035] The seventh aspect of the present invention provides a method for gas-phase epoxidation of propylene, the method comprising: in the presence of a protective gas and a catalyst, mixing hydrogen, oxygen and propylene for reaction to obtain propylene oxide; the catalyst is the titanium silicon molecular sieve loaded with gold nanoparticles catalyst described in the fourth aspect or the titanium silicon molecular sieve loaded with gold nanoparticles catalyst described in the sixth aspect.

[0036] Preferably, the reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1.

[0037] Preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10.

[0038] Preferably, the reaction conditions include: temperature of 100-250° C. and pressure of 0.1-0.7 MPa.

[0039] Preferably, the reaction conditions include: temperature of 120-220° C. and pressure of 0.1-0.5 MPa.

[0040] The inventors of the present invention have found through research that by modifying conventional silicon-titanium molecular sieves, a modified silicon-titanium molecular sieve with weaker acidity and an acid content within a specific range can be obtained, and the modified silicon-titanium molecular sieve with the acid property as a carrier can convert more of the gold nanoparticles loaded thereon into zero valence, and the obtained catalyst can significantly improve the propylene conversion rate in the catalytic propylene gas-phase epoxidation reaction and has a higher propylene oxide selectivity.

[0041] It can be seen from the examples of the present invention that by using the catalyst of the present invention to carry out gas-phase epoxidation of propylene, the propylene conversion rate can be increased to 8-16%, and the propylene oxide selectivity can reach 85-95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 is the NH3-TPD spectra of the modified titanium silicalite molecular sieves prepared in Example A1 and Comparative Example DA1;

[0043] Figure 2 It is the XPS spectra of the catalysts prepared in Example B1 and Comparative Example DB1. DETAILED DESCRIPTION

[0044] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0045] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0046] The first aspect of the present invention provides a modified titanium silicate molecular sieve, wherein the modified titanium silicate molecular sieve has weak acidity and low acid content.

[0047] In the present invention, NH3-TPD is used to detect the acidic function of modified titanium silicalite and other materials. The peak position of the NH3-TPD spectrum is located below 200°C, corresponding to the weak acid position, the peak position of the NH3-TPD spectrum is located at 200-400°C, corresponding to the medium-strong acid position, and the peak position of the NH3-TPD spectrum is located above 400°C, corresponding to the strong acid position. In the present invention, the determination of the NH3-TPD spectrum is carried out on a Micromeritic Autochem 2920 instrument, and the detector is a thermal conductivity detector.

[0048] In the present invention, the peak position of the NH3-TPD spectrum of the modified titanium silicalite is located at 50-200°C, that is, the acidity of the modified titanium silicalite of the present invention is weak acid, there is no medium-strong acid or strong acid, and the acidity is relatively weak.

[0049] In the present invention, the total acid content in the modified titanium silicalite is too high or too low, which is not conducive to the subsequent catalyst prepared for propylene gas phase epoxidation reaction. Specifically, the total acid content of the modified titanium silicalite detected and calculated by NH3-TPD is 0.2-0.5mmol / g, preferably 0.2-0.4mmol / g, such as 0.2mmol / g, 0.24mmol / g, 0.27mmol / g, 0.3mmol / g, 0.32mmol / g, 0.36mmol / g, 0.38mmol / g or 0.4mmol / g.

[0050] In the present invention, the titanium-silicon ratio in the modified titanium silicalite is not particularly limited, and is substantially consistent with the titanium-silicon ratio in the original titanium silicalite before modification. In a preferred embodiment, the molar ratio of titanium to silicon in the modified titanium silicalite may be 0.001-0.04:1, preferably 0.005-0.025:1.

[0051] The inventors have found through research that, in a preferred embodiment, the acid properties of the titanium silicon molecular sieve can be changed by modifying the titanium silicon molecular sieve with a specific substance, thereby obtaining a modified titanium silicon molecular sieve with weaker acidity and lower acid content. Specifically, the modified titanium silicon molecular sieve is obtained by modifying the titanium silicon molecular sieve with nitrate.

[0052] In the present invention, the nitrate used to modify the titanium silicon molecular sieve can be various nitrates well known in the art. In a specific embodiment, the nitrate is selected from one or more of sodium nitrate, potassium nitrate, ammonium nitrate, calcium nitrate, magnesium nitrate, lead nitrate and cerium nitrate. In a preferred embodiment, the nitrate is selected from one or more of potassium nitrate, ammonium nitrate and calcium nitrate.

[0053] In the present invention, the titanium silicalite molecular sieve (original titanium silicalite molecular sieve) used for modification to obtain the modified titanium silicalite molecular sieve can be various types of molecular sieves well known in the art. In a specific embodiment, the titanium silicalite molecular sieve is selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0054] In a specific embodiment, the titanium silicalite molecular sieve used for modification in the present invention is mainly medium-strong acid with less weak acid. The peak position of the NH3-TPD spectrum is located at 50-450°C, and the total acid amount detected and calculated by NH3-TPD is 0.5-0.95mmol / g, wherein the acid amount of weak acid is 0.015-0.15mmol / g, and the acid amount of medium-strong acid is 0.45-0.80mmol / g.

[0055] In the present invention, the titanium-silicon ratio in the modified titanium silicalite is not particularly limited. In a preferred embodiment, the molar ratio of titanium to silicon in the titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:1.

[0056] The second aspect of the present invention provides a method for preparing the modified titanium silicalite described in the first aspect, the method comprising: mixing the titanium silicalite, nitrate and water, and calcining.

[0057] In the method for preparing modified titanium silicalite of the present invention, the weight ratio of the titanium silicalite, nitrate and water can be selected conventionally in the art. In a preferred embodiment, the weight ratio of the titanium silicalite, nitrate and water is 1:0.001-0.2:5-40, preferably 1:0.01-0.15:10-30.

[0058] In the method for preparing modified titanium silicalite of the present invention, in a specific embodiment, the titanium silicalite molecular sieve can be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0059] In a specific embodiment, the peak position of the NH3-TPD spectrum of the titanium silicalite molecular sieve of the present invention is located at 50-450°C, and the total acid amount detected and calculated by NH3-TPD is 0.5-0.95mmol / g, wherein the acid amount of weak acid is 0.015-0.15mmol / g, and the acid amount of medium-strong acid is 0.45-0.80mmol / g.

[0060] In the method for preparing modified titanium silicalite of the present invention, the titanium-silicon ratio in the modified titanium silicalite is not particularly limited. In a preferred embodiment, the molar ratio of titanium to silicon in the titanium silicalite may be 0.001-0.04:1, preferably 0.005-0.025:1.

[0061] In the method for preparing modified titanium silicon molecular sieve of the present invention, the nitrate can be various nitrates well known in the art. In a specific embodiment, the nitrate is selected from one or more of sodium nitrate, potassium nitrate, ammonium nitrate, calcium nitrate, magnesium nitrate, lead nitrate and cerium nitrate. In a preferred embodiment, the nitrate is selected from one or more of potassium nitrate, ammonium nitrate and calcium nitrate.

[0062] In the method for preparing modified titanium silicalite molecular sieve of the present invention, specifically, the method of mixing titanium silicalite molecular sieve, nitrate and water can be a conventional choice in the art, such as mixing and stirring, mixing and ultrasound, etc. Specifically, before roasting, the reaction product obtained by mixing titanium silicalite molecular sieve, nitrate and water is filtered, and then the solid part obtained by filtration is dried at 100-150° C. for 2-5 hours, and then roasted.

[0063] In a specific embodiment, nitrate and water may be prepared into a nitrate aqueous solution, and then the titanium silicon molecular sieve and the nitrate aqueous solution are mixed and treated, and then the reaction product is filtered, and the solid part obtained by filtration is roasted. In a more specific embodiment, the titanium silicon molecular sieve may be added to the nitrate aqueous solution, or the nitrate aqueous solution may be added to the titanium silicon molecular sieve, and then the mixture is mixed and stirred, and the reaction product is filtered, and then the solid part obtained by filtration is roasted.

[0064] In the method for preparing modified titanium silicalite of the present invention, the mixing treatment can be carried out at room temperature. In a specific embodiment, the temperature of the mixing treatment can be 20-80° C., such as 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C. or 80° C. In the method for preparing modified titanium silicalite of the present invention, the mixing time of the mixing treatment can be 0.5-24h, preferably 1-20h, such as 1h, 3h, 5h, 8h, 10, 12h, 15h, 18h or 20h.

[0065] In the method for preparing modified titanium silicon molecular sieve of the present invention, the calcination process can be a conventional operation in the art. In a preferred embodiment, the calcination temperature is 450-650°C, for example, 450°C, 500°C, 550°C, 600°C or 650°C; the calcination time is 4-10h, for example, 4h, 5h, 6h, 7h, 8h, 9h or 10h.

[0066] The third aspect of the present invention provides a modified titanium silicate molecular sieve prepared by the method described in the second aspect. The modified titanium silicate molecular sieve has weak acidity and low acid content, and as a carrier, it can convert more gold nanoparticles loaded thereon into zero valence.

[0067] The fourth aspect of the present invention provides a titanium silicalite supported gold nanoparticle catalyst, the catalyst comprising a carrier and gold nanoparticles supported on the carrier. The carrier is the modified titanium silicalite described in the first aspect or the modified titanium silicalite described in the third aspect, and the gold nanoparticles contain a high proportion of zero-valent Au.

[0068] In a specific embodiment, the proportion of zero-valent Au in the gold nanoparticles is greater than 90% based on the Au element, as determined and calculated by XPS. XPS detection shows that the zero-valent Au (Au 0 ) has a characteristic peak centered at 83-84 eV.

[0069] In the present invention, XPS measurement was performed on an ESCALab250 X-ray photoelectron spectrometer from Thermo Fisher Scientific, with an excitation source of monochromatic Al Kαl X-rays, an energy of 1486.6 eV, and a power of 150 W; the penetration energy used for narrow scanning was 30 eV; the basic vacuum during analysis was about 6.5×10 -8 Pa.

[0070] In the titanium silicon molecular sieve supported gold nanoparticle catalyst of the present invention, in a preferred embodiment, in order to make the catalyst have a higher propylene conversion rate and propylene oxide selectivity when performing propylene gas phase epoxidation reaction, the content of Au element in the catalyst needs to be controlled within an appropriate range. Specifically, based on the gross weight of the catalyst, the content of Au element in the catalyst can be 0.01-1% by weight, preferably 0.04-0.8% by weight, such as 0.04% by weight, 0.06% by weight, 0.1% by weight, 0.2% by weight, 0.3% by weight, 0.4% by weight, 0.5% by weight, 0.6% by weight, 0.7% by weight or 0.8% by weight.

[0071] The titanium silicalite supported gold nanoparticle catalyst of the present invention has a weak acidity of the modified titanium silicalite as a carrier, which is conducive to the gold nanoparticles supported thereon to maintain an electron-filled state, and has a high propylene conversion rate when applied to propylene gas phase epoxidation reaction.

[0072] The fifth aspect of the present invention provides a method for preparing the titanium silicon molecular sieve supported gold nanoparticle catalyst according to the fourth aspect, the method comprising the following steps:

[0073] S1. Mixing a modified titanium silicalite with an aqueous solution of a gold compound, and then adjusting the pH value of the resulting mixture to alkaline, wherein the modified titanium silicalite is the modified titanium silicalite described in the first aspect or the modified titanium silicalite described in the third aspect;

[0074] S2, performing solid-liquid separation on the product obtained in step S1, and activating the obtained solid product.

[0075] In the method for preparing titanium silicon molecular sieve supported gold nanoparticle catalyst of the present invention, the aqueous solution containing gold compound can be a conventional choice in the art. In a specific embodiment, the aqueous solution containing gold compound is selected from one or more of chloroauric acid aqueous solution, cesium chloroaurate aqueous solution and potassium chloroaurate aqueous solution.

[0076] In step S1 of the present invention, mixing the modified titanium silicon molecular sieve with the aqueous solution of the gold compound can be achieved by stirring at room temperature. Similarly, adjusting the pH value of the obtained mixture to alkaline can also be achieved by stirring at room temperature. In a specific embodiment, the process of mixing the modified titanium silicon molecular sieve with the aqueous solution of the gold compound can be: firstly preparing the gold compound aqueous solution with water, and then mixing the modified titanium silicon molecular sieve with the aqueous solution of the gold compound to obtain a mixture. In this article, unless otherwise specified, room temperature refers to 20-30°C.

[0077] In a specific embodiment, in step S1, the concentration of the gold-containing compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, more preferably 0.005-0.05 mol / L, for example, 0.005 mol / L, 0.008 mol / L, 0.01 mol / L, 0.015 mol / L, 0.02 mol / L, 0.025 mol / L, 0.03 mol / L, 0.035 mol / L, 0.04 mol / L, 0.045 mol / L or 0.05 mol / L.

[0078] In step S1 of the present invention, in order to load an appropriate amount of gold nanoparticles on the modified titanium silicon molecular sieve, the amount ratio of the aqueous solution of the gold-containing compound to the modified titanium silicon molecular sieve should be appropriate. In a specific embodiment, in step S1, the amount of the aqueous solution of the gold-containing compound calculated as Au element can be 0.01-5% by weight of the amount of the modified titanium silicon molecular sieve, preferably 0.1-5% by weight, such as 0.1% by weight, 0.5% by weight, 1% by weight, 1.5% by weight, 2% by weight, 2.5% by weight, 3% by weight, 3.5% by weight, 4% by weight, 4.5% by weight or 5% by weight.

[0079] In a specific embodiment, in step S1, the pH value corresponding to the alkalinity may be 7-10, preferably 7-9, such as 7, 7.5, 8, 8.5 or 9. In a specific embodiment, after the pH value of the obtained mixture is adjusted to alkalinity, the obtained product is a suspension.

[0080] In step S1 of the present invention, in a specific embodiment, the pH adjusting agent used to adjust the pH value of the mixture is an alkaline solution. The alkaline solution can be a conventional choice in the art, as long as the pH value of the mixture can be adjusted to alkaline. In a specific embodiment, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

[0081] In step S2 of the present invention, the solid-liquid separation of the product obtained in step S1 may be a solid-liquid separation method well known to those skilled in the art, such as filtration, centrifugation, etc.

[0082] In step S2 of the present invention, the activation process can be a conventional operation in the art. In a specific embodiment, in step S2, the activation conditions include: a temperature of 150-300°C, such as 150°C, 180°C, 200°C, 220°C, 250°C, 280°C or 300°C; a time of 1-5h, such as 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h. In a preferred embodiment, the activation process includes: calcination at 150-300°C for 1-5h in an air atmosphere.

[0083] The sixth aspect of the present invention provides a titanium silicon molecular sieve supported gold nanoparticle catalyst prepared by the method described in the fifth aspect. The catalyst has a large number of zero-valent gold nanoparticles and is used in catalyzing the gas-phase epoxidation reaction of propylene, with a propylene conversion rate of 8-16% and a propylene oxide selectivity of 85-95%.

[0084] The seventh aspect of the present invention provides a method for gas-phase epoxidation of propylene, the method comprising: in the presence of a protective gas and a catalyst, mixing hydrogen, oxygen and propylene for reaction to obtain propylene oxide; the catalyst is the propylene epoxidation catalyst described in the fourth aspect or the propylene epoxidation catalyst described in the sixth aspect.

[0085] In the method for gas-phase epoxidation of propylene of the present invention, under preferred conditions, the reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1; further preferably, the volume flow ratio of propylene and protective gas is 1:1-10.

[0086] In some preferred embodiments of the present invention, the reaction conditions further include: temperature of 100-250° C. and pressure of 0.1-0.7 MPa; further preferably, temperature of 120-200° C. and pressure of 0.1-0.5 MPa.

[0087] In the present invention, the method for gas-phase epoxidation of propylene can be operated in a continuous manner. Specifically, after the catalyst is loaded into the reactor, a mixture of hydrogen, oxygen, propylene and protective gas is continuously added to react. In the present invention, the protective gas can be nitrogen and / or an inert gas.

[0088] The present invention has no special requirements on the form of the catalyst. The catalyst can be titanium silicon molecular sieve loaded with gold nanoparticle powder, or it can be further loaded on a carrier for use. Those skilled in the art can choose according to the type of reactor.

[0089] In the present invention, the separation of the propylene gas-phase epoxidation product and the catalyst can be adjusted according to the form of the catalyst and actual needs. For example, when the catalyst is titanium silicon molecular sieve loaded with gold nanoparticle powder, the product separation and the catalyst recovery and reuse can be achieved by sedimentation, filtration, centrifugation, evaporation, membrane separation and the like; when the catalyst is titanium silicon molecular sieve loaded with gold nanoparticles (molded catalyst) loaded on a carrier, the molten catalyst can be loaded into a fixed bed reactor, and the catalyst can be recovered after the reaction is completed.

[0090] The present invention will be described in detail by way of examples below, but the protection scope of the present invention is not limited thereto. The raw materials used in the following examples are all chemically pure reagents unless otherwise specified. The TS-1 molecular sieve sample used in the examples and comparative examples was prepared according to the method described in the book "Zeolites, 1992, Vol. 12, pages 943-950", and other titanium silicon molecular sieves were commercially available.

[0091] In the examples and comparative examples of the present invention, the acid properties of the titanium silicalite and the modified titanium silicalite were detected and calculated by NH3-TPD. The NH3-TPD spectrum was measured on a Micromeritic Autochem 2920 instrument, and the detector was a thermal conductivity detector.

[0092] In the embodiments and comparative examples of the present invention, the contents of silicon and titanium in the titanium silicalite and modified titanium silicalite were analyzed by X-ray fluorescence spectrometry using a ZSM Primus II X-ray fluorescence spectrometer manufactured by Rigaku Corporation of Japan. The test conditions were a rhodium target, an excitation voltage of 40 kV, and an excitation current of 250 mA.

[0093] In the embodiments and comparative examples of the present invention, the proportion of zero-valent Au in the catalyst is detected and calculated by XPS. XPS measurement is performed on an ESCALab250 X-ray photoelectron spectrometer from Thermo Fisher Scientific, with an excitation source of monochromatic Al Kα X-rays, an energy of 1486.6 eV, and a power of 150 W; the penetration energy used for narrow scanning is 30 eV; the basic vacuum during analysis is about 6.5×10 -8 Pa.

[0094] Examples A1-A6 and comparative examples DA1-DA3 are used to illustrate the preparation process of modified titanium silicalite molecular sieve.

[0095] Example A1

[0096] Calcium nitrate and water were mixed to prepare a calcium nitrate aqueous solution, and then the TS-1 molecular sieve and the calcium nitrate aqueous solution were mixed and stirred at 25°C for 10 hours to obtain a first suspension. After filtering, the solid part was dried at 120°C for 3 hours, and then calcined at 550°C for 6 hours to obtain a modified titanium silicon molecular sieve A1, wherein the molar ratio of titanium to silicon in the TS-1 molecular sieve is 0.015:1, and the weight ratio of the TS-1 molecular sieve, calcium nitrate and water is 1:0.1:20.

[0097] The peak positions of the NH3-TPD spectrum of the TS-1 molecular sieve in Example A1 are located at 93.2°C and 247.5°C. The total acid content detected and calculated by NH3-TPD is 0.596 mmol / g, the weak acid content is 0.081 mmol / g, and the medium-strong acid content is 0.515 mmol / g.

[0098] The peak position of the NH3-TPD spectrum of the modified titanium silicate molecular sieve A1 prepared in Example A1 is located at 93.2°C (eg Figure 1 As shown), the total acid amount detected and calculated by NH3-TPD is 0.298mmol / g, and the weak acid amount is 0.298mmol / g.

[0099] The molar ratio of titanium to silicon in the modified titanium silicalite A1 prepared in Example A1 is 0.015:1.

[0100] Example A2

[0101] Sodium nitrate and water are mixed to prepare a sodium nitrate aqueous solution, and then the TS-2 molecular sieve and the sodium nitrate aqueous solution are mixed and stirred at 40°C for 5 hours to obtain a first suspension. After filtering, the solid part is dried at 120°C for 3 hours, and then calcined at 550°C for 6 hours to obtain a modified titanium silicon molecular sieve A2, wherein the molar ratio of titanium to silicon in the TS-2 molecular sieve is 0.02:1, and the weight ratio of the TS-2 molecular sieve, sodium nitrate and water is 1:0.1:20.

[0102] The peak positions of the NH3-TPD spectrum of the TS-2 molecular sieve in Example A2 are located at 95.6°C and 250.3°C. The total acid content detected and calculated by NH3-TPD is 0.624 mmol / g, the weak acid content is 0.102 mmol / g, and the medium-strong acid content is 0.522 mmol / g.

[0103] The peak position of the NH3-TPD spectrum of the modified titanium silicalite A2 prepared in Example A2 is located at 94.6°C. The total acid content detected and calculated by NH3-TPD is 0.316 mmol / g, and the weak acid content is 0.316 mmol / g.

[0104] The molar ratio of titanium to silicon in the modified titanium silicalite A2 prepared in Example A2 is 0.02:1.

[0105] Example A3

[0106] Magnesium nitrate and water are mixed to prepare a magnesium nitrate aqueous solution, and then the Ti-Beta molecular sieve and the magnesium nitrate aqueous solution are mixed and stirred at 50°C for 12 hours to obtain a first suspension. After filtering, the solid part is dried at 120°C for 3 hours, and then calcined at 550°C for 6 hours to obtain a modified titanium silicon molecular sieve A3, wherein the molar ratio of titanium to silicon in the Ti-Beta molecular sieve is 0.025:1, and the weight ratio of the Ti-Beta molecular sieve, magnesium nitrate and water is 1:0.1:20.

[0107] The peak positions of the NH3-TPD spectrum of the Ti-Beta molecular sieve in Example A3 are located at 99.1 and 248.3°C. The total acid content detected and calculated by NH3-TPD is 0.655 mmol / g, the weak acid content is 0.122 mmol / g, and the medium-strong acid content is 0.533 mmol / g.

[0108] The peak position of the NH3-TPD spectrum of the modified titanium silicalite A3 prepared in Example A3 is located at 97.2°C. The total acid content detected and calculated by NH3-TPD is 0.335 mmol / g, and the weak acid content is 0.335 mmol / g.

[0109] The molar ratio of titanium to silicon in the modified titanium silicalite A3 prepared in Example A3 is 0.025:1.

[0110] Example A4

[0111] Cerium nitrate and water are mixed to prepare a cerium nitrate aqueous solution, and then the Ti-MWW molecular sieve and the cerium nitrate aqueous solution are mixed and stirred at 60°C for 18 hours to obtain a first suspension. After filtering, the solid part is dried at 120°C for 3 hours, and then calcined at 550°C for 8 hours to obtain a modified titanium silicon molecular sieve A4, wherein the molar ratio of titanium to silicon in the Ti-MWW molecular sieve is 0.01:1, and the weight ratio of the Ti-MWW molecular sieve, cerium nitrate and water is 1:0.1:20.

[0112] The peak positions of the NH3-TPD spectrum of the Ti-MWW molecular sieve in Example A4 are located at 90.6 and 250.1°C. The total acid content detected and calculated by NH3-TPD is 0.574 mmol / g, the weak acid content is 0.073 mmol / g, and the medium-strong acid content is 0.501 mmol / g.

[0113] The peak position of the NH3-TPD spectrum of the modified titanium silicalite A4 prepared in Example A4 is located at 92.3°C. The total acid content detected and calculated by NH3-TPD is 0.266 mmol / g, and the weak acid content is 0.266 mmol / g.

[0114] The molar ratio of titanium to silicon in the modified titanium silicalite A4 prepared in Example A4 is 0.01:1.

[0115] Example A5

[0116] Potassium nitrate and water are mixed to prepare a potassium nitrate aqueous solution, and then the TS-1 molecular sieve and the potassium nitrate aqueous solution are mixed and stirred at 70°C for 3 hours to obtain a first suspension. After filtering, the solid part is dried at 120°C for 3 hours, and then calcined at 550°C for 6 hours to obtain a modified titanium silicon molecular sieve A5, wherein the molar ratio of titanium to silicon in the TS-1 molecular sieve is 0.025:1, and the weight ratio of the TS-1 molecular sieve, potassium nitrate and water is 1:0.1:20.

[0117] The peak positions of the NH3-TPD spectrum of the TS-1 molecular sieve in Example A5 are located at 95.5 and 252.3°C. The total acid content detected and calculated by NH3-TPD is 0.670 mmol / g, the weak acid content is 0.134 mmol / g, and the medium-strong acid content is 0.536 mmol / g.

[0118] The peak position of the NH3-TPD spectrum of the modified titanium silicalite A5 prepared in Example A5 is located at 94.5°C. The total acid content detected and calculated by NH3-TPD is 0.357 mmol / g, and the weak acid content is 0.357 mmol / g.

[0119] The molar ratio of titanium to silicon in the modified titanium silicalite A5 prepared in Example A5 is 0.025:1.

[0120] Example A6

[0121] Ammonium nitrate and water were mixed to prepare an aqueous ammonium nitrate solution, and then the TS-1 molecular sieve and the aqueous ammonium nitrate solution were mixed and stirred at 80°C for 15 hours to obtain a first suspension. After filtering, the solid part was dried at 120°C for 3 hours, and then calcined at 550°C for 4 hours to obtain a modified titanium silicon molecular sieve A6, wherein the molar ratio of titanium to silicon in the TS-1 molecular sieve is 0.005:1, and the weight ratio of the TS-1 molecular sieve, ammonium nitrate and water is 1:0.1:20.

[0122] The peak positions of the NH3-TPD spectrum of the TS-1 molecular sieve in Example A6 are located at 94.3 and 250.8°C. The total acid content detected and calculated by NH3-TPD is 0.535 mmol / g, the weak acid content is 0.053 mmol / g, and the medium-strong acid content is 0.482 mmol / g.

[0123] The peak position of the NH3-TPD spectrum of the modified titanium silicalite A6 prepared in Example A6 is located at 96.3°C. The total acid content detected and calculated by NH3-TPD is 0.213 mmol / g, and the weak acid content is 0.213 mmol / g.

[0124] The molar ratio of titanium to silicon in the modified titanium silicalite A6 prepared in Example A6 is 0.005:1.

[0125] Comparative Example DA1

[0126] The TS-1 molecular sieve in Example A1 was directly used without modification and was designated as DA1.

[0127] The peak positions of the NH3-TPD spectrum of TS-1 molecular sieve are located at 93.2 and 247.5℃ (such as Figure 1 As shown), the total acid amount detected and calculated by NH3-TPD is 0.596mmol / g, the weak acid amount is 0.081mmol / g, and the medium-strong acid amount is 0.515mmol / g.

[0128] The molar ratio of titanium to silicon in TS-1 molecular sieve is 0.015:1.

[0129] Comparative Example DA2

[0130] The modified titanium silicalite was prepared by referring to the method described in Green Energy & Environment, 2020, 5(4): 473. The specific process includes:

[0131] 1.0 g of TS-1 molecular sieve powder was added to a solution consisting of 1.5 g of hexadecyl trimethyl ammonium bromide, 210 mL of H2O, 30-160 mL of ethanol, 2.4 mL of ammonia and 0-60 mL of ether. After ultrasonication at 25°C for 10 minutes and stirring for 30 minutes, 1.5 ml of tetraethyl silicate was added dropwise to the solution. The above solution was stirred at 25°C for 6 hours. The final product was centrifuged, washed, dried at 100°C for 12 hours, and finally calcined at 550°C for 6 hours to obtain modified titanium silicon molecular sieve DA2.

[0132] The peak positions of the NH3-TPD spectrum of TS-1 molecular sieve in comparative example DA2 are located at 93.2°C and 247.5°C. The total acid amount detected and calculated by NH3-TPD is 0.596 mmol / g, the weak acid amount is 0.081 mmol / g, and the medium-strong acid amount is 0.515 mmol / g.

[0133] The peak positions of the NH3-TPD spectrum of the modified titanium silicalite DA2 prepared in comparative example DA2 are located at 93.2°C and 247.5°C. The total acid amount detected and calculated by NH3-TPD is 0.391 mmol / g, the weak acid amount is 0.077 mmol / g, and the medium-strong acid amount is 0.314 mmol / g.

[0134] The molar ratio of titanium to silicon in the modified titanium silicalite DA2 prepared in comparative example DA2 is 0.015:1.

[0135] Comparative Example DA3

[0136] The modified titanium silicalite molecular sieve was prepared by referring to the method described in Example 11 of CN102476808A.

[0137] Take 10g TS-1 molecular sieve, 6.2g Al(NO3)3·9H2O and 4.7g magnesium chloride hexahydrate MgCl2·6H2O, add them into a mortar, grind and mix them, then transfer them into a crucible, transfer them into a muffle furnace and calcine them at 550℃ for 4 hours, and recover the product to obtain modified titanium silicon molecular sieve DA3.

[0138] The peak positions of the NH3-TPD spectrum of TS-1 molecular sieve in comparative example DA3 are located at 93.2°C and 247.5°C. The total acid amount detected and calculated by NH3-TPD is 0.596 mmol / g, the weak acid amount is 0.081 mmol / g, and the medium-strong acid amount is 0.515 mmol / g.

[0139] The peak positions of the NH3-TPD spectrum of the modified titanium silicalite DA3 prepared in comparative example DA3 are located at 93.2°C and 247.5°C. The total acid content detected and calculated by NH3-TPD is 0.290 mmol / g, the weak acid content is 0.078 mmol / g, and the medium-strong acid content is 0.212 mmol / g.

[0140] The molar ratio of titanium to silicon in the modified titanium silicalite DA3 prepared in comparative example DA3 is 0.015:1.

[0141] Examples B1-B9 and comparative examples DB1-DB3 are used to illustrate the preparation process of titanium silicalite-supported gold nanoparticle catalysts.

[0142] Example B1

[0143] The modified titanium silicate molecular sieve A1 is mixed with a chloroauric acid aqueous solution to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 3 weight % of the amount of the modified titanium silicate molecular sieve A1, and then a sodium hydroxide solution is added to adjust the pH value of the obtained mixture to 7.7 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B1.

[0144] Example B2

[0145] The modified titanium silicon molecular sieve A2 is mixed with a chloroauric acid aqueous solution to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.05 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 3 weight % of the amount of the modified titanium silicon molecular sieve A2, and then potassium hydroxide solution is added to adjust the pH value of the obtained mixture to 8.1 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B2.

[0146] Example B3

[0147] The modified titanium silicate molecular sieve A3 is mixed with a chloroauric acid aqueous solution to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.08 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 3 weight % of the amount of the modified titanium silicate molecular sieve A3, and then a cesium hydroxide solution is added to adjust the pH value of the obtained mixture to 8 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B3.

[0148] Example B4

[0149] The modified titanium silicon molecular sieve A4 is mixed with an aqueous solution of chloroauric acid to obtain a mixture, wherein the concentration of the aqueous solution of chloroauric acid is 0.005 mol / L, and the amount of the aqueous solution of chloroauric acid used in terms of Au element is 3 weight % of the amount of the modified titanium silicon molecular sieve A4, and then urea solution is added to adjust the pH value of the obtained mixture to 7.5 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B4.

[0150] Example B5

[0151] The modified titanium silicate molecular sieve A5 is mixed with a chloroauric acid aqueous solution to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.008 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 3 weight % of the amount of the modified titanium silicate molecular sieve A5, and then a sodium bicarbonate solution is added to adjust the pH value of the obtained mixture to 7.4 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B5.

[0152] Example B6

[0153] The modified titanium silicon molecular sieve A6 is mixed with a chloroauric acid aqueous solution to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.01 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 3 weight % of the amount of the modified titanium silicon molecular sieve A6, and then potassium carbonate solution is added to adjust the pH value of the obtained mixture to 7.5 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B6.

[0154] Example B7

[0155] The modified titanium silicate molecular sieve A1 is mixed with a chloroauric acid aqueous solution to obtain a mixture, wherein the concentration of the chloroauric acid aqueous solution is 0.09 mol / L, and the amount of the chloroauric acid aqueous solution calculated as Au element is 4.5% by weight of the amount of the modified titanium silicate molecular sieve A1, and then potassium bicarbonate solution is added to adjust the pH value of the obtained mixture to 7.8 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B7.

[0156] Example B8

[0157] The modified titanium silicate molecular sieve A1 is mixed with an aqueous solution of chloroauric acid to obtain a mixture, wherein the concentration of the aqueous solution of chloroauric acid is 0.0008 mol / L, and the amount of the aqueous solution of chloroauric acid used in terms of Au element is 0.05 weight % of the amount of the modified titanium silicate molecular sieve A1, and then a cesium carbonate solution is added to adjust the pH value of the obtained mixture to 7.6 to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, calcination at 200°C for 2h to obtain catalyst B8.

[0158] Example B9

[0159] The modified titanium silicate molecular sieve A1 is mixed with an aqueous solution of chloroauric acid to obtain a mixture, wherein the concentration of the aqueous solution of chloroauric acid is 0.03 mol / L, and the amount of the aqueous solution of chloroauric acid used in terms of Au element is 3 weight % of the amount of the modified titanium silicate molecular sieve A1, and then the pH value of the obtained mixture is adjusted to 9.1 with a sodium carbonate solution to obtain a second suspension; then the second suspension is filtered, and the obtained filter residue is activated, and the activation conditions include: air atmosphere, roasting at 200°C for 2h to obtain catalyst B9.

[0160] Comparative Example DB1

[0161] The method of Example B1 is followed, except that the modified titanium silicalite A1 is replaced by modified titanium silicalite DA1 to obtain catalyst DB1.

[0162] Comparative Example DB2

[0163] The method of Example B1 is followed, except that the modified titanium silicalite A1 is replaced by modified titanium silicalite DA2 to obtain catalyst DB2.

[0164] Comparative Example DB3

[0165] The method of Example B1 was followed, except that the modified titanium silicalite A1 was replaced by modified titanium silicalite DA3 to obtain catalyst DB3.

[0166] Test Example 1

[0167] The content of Au element in the catalysts B1-B9 and DB1-DB3 prepared in Examples B1-B9 and Comparative Examples DB1-DB3 was tested, and the results are shown in Table 1. The test method is: according to the ASTM D5185 standard method, using SPECTRO ACROSS inductively coupled plasma (ICP) for determination.

[0168] XPS was used to detect the characteristic peak positions of Au elements in the catalysts B1-B9 and DB1-DB3 prepared in Examples B1-B9 and Comparative Examples DB1-DB3, and the proportion of zero-valent Au was calculated. The results are shown in Table 1. The spectra of the catalysts prepared in Example B1 and Comparative Example DB1 are shown in Table 1. Figure 2 shown.

[0169] Table 1

[0170] serial number Au element content / wt% Au element characteristic peak position / eV Percentage of zero-valent Au / % Example B1 0.71 83.55 93.5 Example B2 0.78 83.61 91.2 Example B3 0.82 83.75 90.3 Example B4 0.62 83.31 93.8 Example B5 0.65 83.42 93.2 Example B6 0.67 83.37 92.8 Example B7 0.88 83.86 90.1 Example B8 0.14 83.26 94.2 Example B9 0.76 83.51 93.4 Comparative Example DB1 0.70 84.55 70.2 Comparative Example DB2 0.71 84.13 65.1 Comparative Example DB3 0.71 84.23 67.6

[0171] Test Example 2

[0172] This test example is used to illustrate the reaction effect of catalysts B1-B9 and DB1-DB3 prepared by Examples B1-B9 of the present invention and Comparative Examples DB1-DB3 for gas-phase epoxidation of propylene. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The instrument used is a 6890 gas chromatograph produced by Agilent, molecular sieve 5A and PoraBOND U chromatographic columns, FID and TCD detectors.

[0173] In each embodiment and comparative example:

[0174] Propylene conversion % = (the number of moles of propylene in the feedstock - the number of moles of propylene in the product) / the number of moles of propylene in the feedstock × 100%;

[0175] Propylene oxide selectivity % = number of moles of propylene oxide in the product / total number of moles of the product × 100%.

[0176] The test process is as follows: the catalyst samples prepared in the above-mentioned embodiment and comparative example are taken respectively, loaded into a tubular reactor with an inner diameter of 8 mm, then heated to 180°C in a N2 atmosphere, and hydrogen, oxygen and propylene are introduced to start the reaction. After the reaction for 1 hour, the product is analyzed online; wherein, the amount of catalyst is 0.4 g, the flow rates of hydrogen, oxygen, propylene and nitrogen are 2 mL / min, 2 mL / min, 2 mL / min and 14 mL / min respectively, the reaction pressure is 0.1 MPa, and the catalytic reaction results are shown in Table 2.

[0177] Table 2

[0178] serial number Propylene conversion rate / % Propylene oxide selectivity / % Example B1 13.5 90.3 Example B2 12.5 91.2 Example B3 12.8 92.3 Example B4 13.8 90.1 Example B5 12.5 93.5 Example B6 12.9 89.4 Example B7 10.3 85.2 Example B8 8.5 93.6 Example B9 11.7 90.5 Comparative Example DB1 5.6 88.6 Comparative Example DB2 4.5 83.2 Comparative Example DB3 5.1 82.3

[0179] As can be seen from Table 2, the propylene conversion rate of the catalyst provided in the embodiment of the present invention for the propylene gas-phase epoxidation reaction is significantly higher than that of the comparative example, and the propylene oxide selectivity of the catalyst provided in the embodiment of the present invention for the propylene gas-phase epoxidation reaction is also maintained at a high level.

[0180] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A modified titanium silicon molecular sieve, characterized in that: The peak position of the NH3-TPD spectrum of the modified titanium silicalite is located at 50-200°C, and the total acid content detected and calculated by NH3-TPD is 0.2-0.5 mmol / g, preferably 0.2-0.4 mmol / g.

2. The modified titanium silicon molecular sieve according to claim 1, characterized in that: The molar ratio of titanium to silicon in the modified titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:

1.

3. The modified titanium silicon molecular sieve according to claim 1 or 2, characterized in that: The modified titanium silicate molecular sieve is obtained by modifying the titanium silicate molecular sieve with nitrate.

4. The modified titanium silicon molecular sieve according to any one of claims 1 to 3, characterized in that: The nitrate is selected from one or more of sodium nitrate, potassium nitrate, ammonium nitrate, calcium nitrate, magnesium nitrate, lead nitrate and cerium nitrate.

5. The modified titanium silicon molecular sieve according to any one of claims 1 to 4, characterized in that: The titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve; Preferably, the peak position of the NH3-TPD spectrum of the titanium silicalite molecular sieve is located at 50-450°C, and the total acid amount detected and calculated by NH3-TPD is 0.5-0.95 mmol / g, wherein the acid amount of weak acid is 0.015-0.15 mmol / g, and the acid amount of medium-strong acid is 0.45-0.80 mmol / g; Preferably, the molar ratio of titanium to silicon in the titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:

1.

6. A method for preparing the modified titanium silicon molecular sieve according to any one of claims 1 to 5, characterized in that: The method comprises: mixing titanium silicon molecular sieve, nitrate and water, and roasting.

7. The method according to claim 6, characterized in that The weight ratio of the titanium silicate molecular sieve, nitrate and water is 1:0.005-0.2:5-40, preferably 1:0.01-0.15:5-30.

8. The method according to claim 6 or 7, characterized in that: The titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve; Preferably, the peak position of the NH3-TPD spectrum of the titanium silicalite molecular sieve is located at 50-450°C, and the total acid amount detected and calculated by NH3-TPD is 0.5-0.95 mmol / g, wherein the acid amount of weak acid is 0.015-0.15 mmol / g, and the acid amount of medium-strong acid is 0.45-0.80 mmol / g; Preferably, the molar ratio of titanium to silicon in the titanium silicalite is 0.001-0.04:1, preferably 0.005-0.025:

1.

9. The method according to any one of claims 6 to 8, characterized in that: The nitrate is selected from one or more of sodium nitrate, potassium nitrate, ammonium nitrate, calcium nitrate, magnesium nitrate, lead nitrate and cerium nitrate.

10. The method according to any one of claims 6 to 9, characterized in that: The mixing treatment conditions include: the mixing treatment method is mixed stirring; the mixing treatment temperature is 20-80° C.; the mixing treatment time is 0.5-24 h, preferably 1-20 h.

11. The method according to any one of claims 6 to 10, characterized in that: The calcination conditions include: calcination temperature of 450-650° C.; calcination time of 4-10 hours.

12. A modified titanium silicalite molecular sieve prepared by the method according to any one of claims 6 to 11.

13. A titanium silicon molecular sieve supported gold nanoparticle catalyst, characterized in that: The catalyst comprises a carrier and gold nanoparticles loaded on the carrier, Calculated on the basis of Au element, the proportion of zero-valent Au in the gold nanoparticles is greater than 90%, as determined and calculated by XPS; The carrier is the modified titanium silicate molecular sieve according to any one of claims 1 to 5 or the modified titanium silicate molecular sieve according to claim 12.

14. The catalyst according to claim 13, characterized in that Based on the total weight of the catalyst, the content of Au element in the catalyst is 0.01-1% by weight, preferably 0.04-0.8% by weight.

15. A method for preparing the titanium silicon molecular sieve supported gold nanoparticle catalyst according to claim 13 or 14, characterized in that: The method comprises the following steps: S1, mixing the modified titanium silicon molecular sieve with an aqueous solution of a gold compound, and then adjusting the pH value of the resulting mixture to alkaline; S2, performing solid-liquid separation on the product obtained in step S1, and activating the obtained solid product; The modified titanium silicate molecular sieve is the modified titanium silicate molecular sieve described in any one of claims 1 to 5 or the modified titanium silicate molecular sieve described in claim 12.

16. The method according to claim 15, characterized in that The gold compound aqueous solution is selected from one or more of a chloroauric acid aqueous solution, a cesium chloroaurate aqueous solution and a potassium chloroaurate aqueous solution.

17. The method according to claim 15 or 16, characterized in that In step S1, the concentration of the gold compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

18. The method according to any one of claims 15 to 17, characterized in that: In step S1, the amount of the gold-containing compound aqueous solution calculated as Au element is 0.01-5% by weight, preferably 0.1-5% by weight, of the amount of the modified titanium silicon molecular sieve.

19. The method according to any one of claims 15 to 18, characterized in that: In step S1, the pH value of the mixture is adjusted to 7-10, preferably 7-9.

20. The method according to any one of claims 15 to 19, characterized in that: In step S1, the pH adjusting agent used to adjust the pH value of the mixture is an alkaline solution; Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

21. The method according to any one of claims 15 to 20, characterized in that: In step S2, the activation conditions include: temperature of 150-300°C and time of 1-5h.

22. A titanium silicalite-supported gold nanoparticle catalyst prepared by the method according to any one of claims 15 to 21.

23. A method for gas phase epoxidation of propylene, characterized in that: The method comprises: mixing hydrogen, oxygen and propylene for reaction in the presence of protective gas and catalyst to obtain propylene oxide; The catalyst is the titanium silicon molecular sieve supported gold nanoparticle catalyst as described in any one of claims 13, 14 or 22.

24. The method according to claim 23, characterized in that The reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1; Preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10.

25. The method according to claim 23 or 24, characterized in that The reaction conditions include: temperature of 100-250°C and pressure of 0.1-0.7MPa; Preferably, the reaction conditions include: temperature of 120-220° C. and pressure of 0.1-0.5 MPa.

Citation Information

Patent Citations

  • Modified titanium silicate molecular sieve material and preparation method thereof

    CN102476808A

  • Nanosized gold catalyst used for preparing propylene oxide by direct propylene oxidation and preparation method thereof

    CN101530814A

  • Modified titanium silicalite molecular sieve and modifying method and application

    CN106115732A

  • Metal oxide / HTS-1 titanium silicalite molecular sieve catalyst and preparation method and application thereof