Forming method for improving structure uniformity of TC11 titanium alloy by using broaching machine

Through the axial forging, punching and horse frame expansion of the TC11 titanium alloy forgings through a reaming machine, combined with heat treatment and mechanical processing, the problem that the uniformity of the titanium alloy structure is difficult to meet the requirements is solved, and an efficient and uniform titanium alloy is achieved. Production of forgings for demanding applications in the aerospace sector.

CN118768501APending Publication Date: 2024-10-15SHAANXI HONGYUAN AVIATION FORGING
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410899537.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The structural uniformity of TC11 titanium alloy before hot forming is difficult to meet product requirements. The existing forging process is complex and energy-consuming, and small-volume titanium alloys are widely used in the aviation field. The uniformity needs to be judged through comprehensive microstructure observation.

Method used

A hole expansion machine is used for uniform rolling. Through axial forging, center punching and horse frame expansion, combined with heat treatment and mechanical processing, the heating temperature, deformation amount and operating level of the forging are controlled, and dynamic recrystallization generates uniform grains.

Benefits of technology

It improves the uniformity of the internal structure of forgings, meets the high requirements for titanium alloys in the aviation field, reduces production fire times and energy consumption, and improves production efficiency and thermal effect control.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of metal material internal structure forming, and particularly relates to a forming method for improving TC11 titanium alloy structure uniformity through a broaching machine. Comprising the steps that 1, the inner diameter, the outer diameter and the height of an annular tire film are determined; 2, in the annular tire mold, the bar is subjected to axial forging, and a cake blank with the height size of the tire mold is obtained; 3, center punching and trestle chambering are sequentially conducted on the cake blank to obtain a preformed blank, and the center punching process and trestle chambering are conducted under the following technological conditions that the heating standard is that the temperature is 35-40 DEG C under the phase transformation point, the heating coefficient is 0.9-0.85 min / mm, the heating equipment is an electric furnace, the hammering frequency is 2.0-3.0 s / hammer, air cooling is conducted, and one heating number is achieved; and 4, the preformed blank is subjected to chambering forming, and an intermediate blank is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of internal structure forming of metal materials, and in particular relates to a forming method for improving the uniformity of the structure of a TC11 titanium alloy by using a hole expander. Background Art

[0002] The TC11 titanium alloy raw material is melted with titanium liquid cotton, blanked, and forged into bars. The uniformity of the structure is difficult to meet the requirements of the required products. Therefore, before hot forming the products, forging equipment is needed to homogenize the forgings to meet the product requirements.

[0003] At present, most manufacturers use hydraulic presses to carry out uniform forging of titanium alloys, and only judge the uniformity of the forgings by the transverse surface microstructure of the forgings. In reality, small-volume TC11 titanium alloys are widely used in the aviation field, and the uniformity of the forgings is required to be higher. It is necessary to comprehensively judge the uniformity of the forgings by water immersion flaw detection and transverse and longitudinal microstructure observation.

[0004] The TC11 forgings produced by the 3T free forging hammer have complex forging steps, many production times, high labor intensity, high proficiency requirements, long production cycle, high energy consumption and other defects. In order to improve production efficiency, reduce production times, and make full use of equipment to streamline the production process, the TC11 billet rings are effectively improved first, and the method of membrane forging and reaming machine reaming is used to effectively improve the production efficiency of forgings and the required internal organization qualification rate, and at the same time, the thermal effect of forgings can be well controlled. By comprehensively considering the heating temperature, deformation, forging times and operation level of the forgings, the uniformity of the forgings can be improved by uniformly rolling the billet using the reaming machine equipment. Summary of the invention

[0005] Purpose of the invention: To provide a forming method for improving the uniformity of the microstructure of TC11 titanium alloy by using a hole expander so that it can meet the required internal microstructure and flaw detection requirements.

[0006] Technical solution:

[0007] A forming method for improving the uniformity of the structure of TC11 titanium alloy by using a hole expander, the method is used for forming a ring, and the method comprises:

[0008] Step 1: Determine the inner diameter, outer diameter and height of the annular fetal membrane;

[0009] Step 2: In the annular fetal membrane, the rod is axially forged to obtain a cake blank with a fetal membrane height size;

[0010] Step 3: The preform is sequentially subjected to center punching and horse rack expansion to obtain a preform, wherein the center punching process and the horse rack expansion process are both carried out under the following process conditions: heating specification: 35°C to 40°C below the phase change point, heating coefficient: 0.9min / mm to 0.85min / mm, heating equipment: electric furnace, hammering frequency: 2.0 to 3.0s / hammer, air cooling, one fire;

[0011] Step 4: Expand the preform to obtain an intermediate blank.

[0012] Furthermore, step 1 also includes: heat treating and machining the fetal membrane, wherein the preheating temperature is 250°C to 300°C, and the surface roughness of the inner hole and end face of the fetal membrane after machining is Ra3.2, and the surface roughness of the rest is Ra6.3.

[0013] Furthermore, step 1 specifically includes:

[0014] The inner diameter of the fetal membrane satisfies that the volume of the fetal membrane cavity is 1.1% larger than the required ring volume. The outer diameter of the fetal membrane exceeds the inner diameter of the fetal membrane by 50mm to 75mm while meeting the conventional forging strength. The height H of the fetal membrane is 1.1 to 1.05 times the required ring height H.

[0015] Furthermore, in step 2, the heating specification is: 20°C~25°C below the phase change point, the heating coefficient is: 1.0min / mm~0.9min / mm, the heating equipment is: electric furnace, the deformation amount is: 25%~40%, the hammering frequency is: 2~3.5s / hammer, air cooling, 1 fire.

[0016] Furthermore, in step 3, the height h of the punching core material of the center punching is 1 / 3 to 1 / 3.5 times the required ring height H; the aperture size of the punching core material is 1 / 3 of the volume material of the required ring with the same height.

[0017] Furthermore, in step 3, the size of the horse frame expansion hole meets the following requirements: the height is the height of the fetal membrane, and the inner diameter is set to a deformation amount of 35% to 45% under the premise of ensuring the deformation amount of the final forming of the forging.

[0018] Furthermore, in step 4, the specific process parameters are: 40°C to 45°C below the phase change point, heating coefficient: 0.8min / mm to 0.85min / mm, heating equipment: electric furnace, deformation: 40% to 45%, hole expansion rate: 5mm / s to 6mm / s, air cooling, and production is completed in one fire.

[0019] Furthermore, in step 3, the deformation amount during the expansion process is 30% to 35%.

[0020] Beneficial effects: The present invention uses an electro-hydraulic hammer to perform bidirectional free forging of bars at a relatively high temperature, which can effectively improve the long strip and short rod α phase of the raw material. By directly controlling the heating temperature, deformation, forging fire and operation level of the forging during the production process, the dynamic recrystallization of the forging is indirectly used to generate uniform grains, and a primary equiaxed α phase with a content of about 35%-40% is generated at the grain boundary, thereby improving the overall uniformity of the forging structure. DETAILED DESCRIPTION

[0021] The present invention utilizes a hole expander to produce forgings whose blanks are rings, so that they meet the required internal organization and flaw detection requirements. The required internal organization is: low-power conformity equiaxed fuzzy crystals, the α content of the transverse and longitudinal microstructures is 15% to 50%, and is equiaxed α, without elongated or blocky α. Flaw detection requirements: φ0.6mm flat bottom hole, half sound path, clutter reflection signal ≤30%, bottom loss change ≤50%.

[0022] The present invention provides a forming method for improving the uniformity of the TC11 titanium alloy structure by using a hole expander, the method comprising the following steps:

[0023] Step 1: pre-set a fetal membrane that meets the required height of the intermediate blank: the inner diameter of the fetal membrane meets the requirement that the fetal membrane cavity volume is 1.1% larger than the required ring volume; the outer diameter of the fetal membrane exceeds the inner diameter of the fetal membrane by 50mm to 75mm while meeting the conventional forging strength; the height H of the fetal membrane is 1.1 to 1.05 times the required ring height H; the fetal membrane needs to be heat treated and machined before use, and its internal control and end surface roughness requirements are Ra3.2; the rest are Ra6.3; the fetal membrane needs to be preheated before use: the preheating temperature is 250℃ to 300℃:

[0024] Step 2, axially upsetting the bar to obtain a blank, heating specification: 20°C to 25°C below the phase change point, heating coefficient: 1.0min / mm to 0.9min / mm, heating equipment: electric furnace, deformation: 25% to 40%, hammering frequency: 2 to 3.5s / hammer, air cooling, 1 fire, axially forging to the blank with the height of the fetal membrane in the pre-set above-mentioned fetal membrane;

[0025] Step 3: center punch and expand the blank obtained in step 2, set a reasonable preform for the expansion in step 3, heating specification: 35℃~40℃ below the phase change point, heating coefficient: 0.9min / mm~0.85min / mm, heating equipment: electric furnace, expansion deformation: 30%~35%, hammering frequency: 2.0~3.0s / hammer, air cooling, one fire. The size of the center punch and the expansion is set according to the final forming size of the ring, and the center punch and the expansion are completed in one fire;

[0026] Center punching: The height h of the punching core material is 1 / 3 to 1 / 3.5 times the required ring height H; the diameter of the center punching hole can be 1 / 3-1 / 3.5 of the volume of the required ring with the same height;

[0027] The size of the horse frame expansion hole; the height is 1.1 to 1.05 times the required height of the forging, that is, the same as the height of the fetal membrane; the inner diameter size is set to 35% to 45% under the premise of ensuring the deformation of the final forging: the outer diameter size will naturally produce the outer diameter size when the height and inner diameter are determined according to the equal volume principle;

[0028] Step 4, expand the blank obtained in step 3, heating specification: 40℃~45℃ below phase change point, heating coefficient: 0.8min / mm~0.85min / mm, heating equipment: electric furnace, deformation: 40%~45%, expansion rate: 5mm / s~6mm / s, air cooling, and one fire to complete the production.

[0029] The above-mentioned forming method using a hole expander to improve the uniformity of the TC11 titanium alloy structure has the characteristics of pulse loading according to the characteristics of the production equipment, resulting in obvious thermal effects in the core of the forging during forging production, and it is necessary to reasonably control variables such as the forging temperature, forging frequency and deformation amount of the forging.

[0030] The above-mentioned forming method using a hole expansion machine to improve the uniformity of the TC11 titanium alloy structure, under the condition of suitable forging frequency (hammer frequency and hole expansion rate), different forging temperatures need to strictly match different forging deformation amounts, and different forging temperatures can only perform 1 upsetting forging, 1 punching and expansion forging, and 1 hole expansion forming. A total of 3 fires were completed;

[0031] 1. The upsetting forging adopts a special tire membrane to control the deformation of the forging; 1. The punching and expansion forging adopts the setting of the preforming size to control the deformation; 1. The expansion forming adopts the setting of the ring speed increase to control the deformation; The deformation is controlled by different equipment, so that the desired internal part is finally obtained to achieve the purpose of Tc11 forging;

[0032] The above-mentioned forming method using a hole expansion machine to improve the uniformity of the TC11 titanium alloy structure requires a combination of membrane forging, reaming forging and hole expansion forging to improve the overall uniformity of the forging and meet the standard requirements because the raw material has unqualified structures evenly distributed on the substrate.

[0033] The above-mentioned forming method using a hole expander to improve the uniformity of the TC11 titanium alloy structure requires forming at a temperature above the dynamic recrystallization end temperature and below the phase transformation point, that is, 40°C-45°C below the phase transformation point, so that the forging can achieve the purpose of overall structural uniformity with the least number of fires.

[0034] In the above-mentioned forming method using a hole expander to improve the uniformity of the TC11 titanium alloy structure, the forging temperature is a decreasing process, and the structural change also forms a slow-changing condition, which will not cause grain unevenness. The primary α phase morphology finally formed at the grain boundary meets the equiaxed requirements and the content is in the range of 35%-50%.

[0035] Embodiment 1:

[0036] Part number: XX52852FG; Cutting specifications: φ230×135; Weight: 25.2Kg; Required blank size: φ400±3×φ300±1×75±1;

[0037] Step 1: pre-set a fetal membrane that meets the height required for the intermediate blank forming; the fetal membrane size is φ400±3×φ295±1×80±1; the inner circle mold slope is 3°, and the end face chamfer is R10;

[0038] Step 2: After heating in an electric furnace at Tβ-25℃×160min, forging deformation: 32%, hammering frequency: 2.5s / hammer, cooling method: air cooling, production fire: 1 fire completed;

[0039] Step 3: Heat the φ230×135 bar material; produce it on a 3T free forging hammer using the pre-set membrane axial upsetting and punching; upsetting cake size: ~Φ295×80±3; use the pre-set membrane upsetting cake and then punch the center hole Φ90; punching core material ≤Φ90×30 (~≤1.0Kg) horse rack expansion, flat end face to rough size: ~Φ335×Φ170±5×80-+12; horse expansion deformation: 32%, hammer frequency: 2..6s / hammer, cooling method is air cooling, production fire is completed in 1 job;

[0040] Step 4, expand the hole of the horse frame and flatten the end surface to the rough size: ~Φ335×Φ170±5×80-+12, heat at Tβ-40℃×175min, and use a Φ1200mm expansion machine with equipment number 4505002 to expand; the expanded size is: φ408±3×φ292±3×80±2; expansion deformation: 43%, expansion rate: 5.5mm / s, cooling method air cooling, production fire number: one fire completed.

[0041] Step 5, machining: uniform machining of the upper and lower end faces and inner circle; single-sided machining amount ≤ 2.5mm; surface roughness Ra1.6; machining dimensions: φ400±1×φ300±1×75±1; end face chamfer R5;

[0042] Step 6: Corrosion is performed on both sides 100% according to the standard of HB5262;

[0043] Step 7, flaw detection: Ultrasonic flaw detection is carried out according to HB5262 standard;

[0044] Step 8. Physical and chemical: Check at high magnification.

[0045] Comprehensively judging, the TC11 titanium alloy forgings prepared in this embodiment are uniform as a whole, meet the marking requirements, and are qualified after testing.

[0046] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent changes made to the above embodiments according to the technical essence of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A forming method for improving the uniformity of TC11 titanium alloy structure by using a hole expander, characterized in that: The method is used for forming a ring, and the method comprises: Step 1: Determine the inner diameter, outer diameter and height of the annular fetal membrane; Step 2: In the annular fetal membrane, the rod is axially forged to obtain a cake blank with a fetal membrane height size; Step 3: The preform is sequentially subjected to center punching and horse rack expansion to obtain a preform, wherein the center punching process and the horse rack expansion process are both carried out under the following process conditions: heating specification: 35°C to 40°C below the phase change point, heating coefficient: 0.9min / mm to 0.85min / mm, heating equipment: electric furnace, hammering frequency: 2.0 to 3.0s / hammer, air cooling, one fire; Step 4: Expand the preform to obtain an intermediate blank.

2. The method according to claim 1, characterized in that Step 1 also includes: heat treatment and mechanical processing of the fetal membrane, wherein the preheating temperature is 250°C to 300°C, and the surface roughness of the inner hole and end face of the fetal membrane after machining is Ra3.2, and the surface roughness of the rest is Ra6.

3.

3. The method according to claim 1, characterized in that: Step 1 specifically includes: The inner diameter of the fetal membrane satisfies: the volume of the fetal membrane cavity is 1.1% larger than the required ring volume; the outer diameter of the fetal membrane exceeds the inner diameter of the fetal membrane by 50mm to 75mm while meeting the conventional forging strength; the height H of the fetal membrane is 1.1 to 1.05 times the required ring height H.

4. The method according to claim 1, characterized in that: In step 2, the heating specification is: 20℃~25℃ below the phase change point, the heating coefficient is: 1.0min / mm~0.9min / mm, the heating equipment is: electric furnace, the deformation is: 25%~40%, the hammering frequency is: 2~3.5s / hammer, air cooling, 1 fire.

5. The method according to claim 4, characterized in that In step 3, the height h of the punching core material of the center punching is 1 / 3 to 1 / 3.5 times the required ring height H; the aperture size of the punching core material is 1 / 3-1 / 3.5 of the volume material of the required ring with the same height.

6. The method according to claim 1, characterized in that In step 3, the size of the horse frame expansion hole meets the following requirements: the height is the height of the fetal membrane, and the inner diameter is set to a deformation amount of 35% to 45% under the premise of ensuring the deformation amount of the final forming of the forging.

7. The method according to claim 1, characterized in that In step 4, the specific process parameters are: 40°C to 45°C below the phase change point, heating coefficient: 0.8min / mm to 0.85min / mm, heating equipment: electric furnace, deformation: 40% to 45%, hole expansion rate: 5mm / s to 6mm / s, air cooling, and one-fire production.

8. The method according to claim 1, characterized in that In step 3, the deformation amount during the expansion process is 30% to 35%.

Citation Information

Patent Citations

  • High-temperature alloy disc die forging method

    CN104707929A

  • Forging method for improving structural steel large annular piece flaw detection

    CN108237197A

  • Metal ring piece forging size control method

    CN108856613A

  • Forming method of 718 plus special-shaped ring forge piece

    CN109530607A

  • Method for obtaining uniform structure for TC11 titanium alloy round cake billet

    CN109622839A