Shell structure die-casting forming method

By using semi-solid aluminum alloy slurry and controlling the advancement speed and pressure in stages during the die-casting process, the problems of rapid solidification of liquid metal and introduction of impurities are solved, efficient die-casting of the shell structure is achieved, and the accuracy and productivity of the finished product are improved. .

CN118768540AInactive Publication Date: 2024-10-15LPAC MASCH (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310357270.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the die-casting process, the rapid solidification of liquid metal and the introduction of impurities lead to a decline in product performance, and conventional methods are difficult to ensure air removal and metal fluidity in the mold cavity, affecting molding quality and efficiency.

Method used

Semi-solid aluminum alloy slurry is used to advance through the preheated mold and quantitative pump, and the advancement speed and pressure are controlled in stages to ensure that the aluminum alloy slurry fully fills the mold cavity, and heat treatment is performed to improve the molding quality.

Benefits of technology

It shortens the solidification time, lowers the processing temperature, improves the dimensional accuracy and productivity of the finished product, reduces the subsequent processing process and cost, and improves the molding rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a shell structure die-casting forming method which comprises the following steps: 1, screening, crushing, purifying, activating, micronizing and disinfecting natural zeolite to obtain zeolite particles; 2, weighing zeolite particles, pouring the zeolite particles into a mixing machine, weighing bentonite, activated carbon and water, and mixing in the mixing machine; 3, adding the prepared mixture into a shot blasting machine to prepare beaded zeolite large particles; and 4, drying the prepared large beaded zeolite particles, and roasting to prepare the zeolite alcoholization decanting beads. According to the zeolite alcoholization decanting bead processed by the method, through the natural adsorption, catalysis, ion exchange and other functions of zeolite, under the condition that a finished wine product is unsealed, the esterification reaction of alcohols and acids in the wine product is accelerated through catalysis, rapid conversion from new wine to aged wine is achieved, the taste is greatly enhanced, and the effect of dispelling the effects of alcohol and acid in the wine product is achieved. And the fragrance of the wine is more savoury and mellow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of die casting, in particular to a shell structure die casting method. Background Art

[0002] Die casting is a metal casting process characterized by the use of high pressure to apply molten metal to the mold cavity. The mold is usually made of a stronger alloy and the process is somewhat similar to injection molding. Most die castings are non-ferrous, such as zinc, copper, aluminum, magnesium, lead, tin, lead-tin alloys and their alloys. Depending on the type of die casting, a cold chamber die casting machine or a hot chamber die casting machine is required.

[0003] In conventional liquid molding, due to the high injection speed, the liquid easily forms turbulence in the mold cavity, and the air in the mold cavity is drawn into the product; the temperature difference is large when the liquid hits the mold, and the liquid on the surface solidifies quickly, which increases the flow resistance of the core liquid, so it cannot be well fused to form a cold shut. At the same time, the alloy introduces oxides or some other impurities during the smelting and casting process, which eventually leads to reduced product performance.

[0004] Therefore, those skilled in the art provide a shell structure die-casting method to solve the problems raised in the above background technology. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a shell structure die-casting method, comprising the following steps.

[0006] S1: Customize the casting mold and process the corresponding casting mold according to the structural design of the shell;

[0007] S2: preparing metal raw materials, taking aluminum alloy raw materials and putting them into a machine-side furnace for smelting, and putting the molten metal into a pulping machine after smelting to obtain semi-solid aluminum alloy slurry;

[0008] S3: preheating the mold to 250-350°C;

[0009] S4: spraying a release agent onto the surfaces of the concave and convex molds of the preheated mold, and then closing the mold;

[0010] S5: Use a quantitative pump to deliver the prepared semi-solid metal into the die-casting machine, and squeeze the die-casting machine punch to push the semi-solid metal into the mold; the pushing is divided into three stages. In the first stage, the pushing is carried out at a low speed so that the aluminum alloy slurry slowly passes through the inner gate; in the second stage, the pushing speed is increased so that the aluminum alloy slurry is quickly filled into the mold cavity; in the third stage, the pushing speed is reduced so that the aluminum alloy slurry is fully filled into the mold cavity, and the casting is completed in combination with the pressurization treatment to obtain the casting blank;

[0011] S6: Heat treatment: heat-treating the above casting blank to obtain a casting product.

[0012] Preferably, in step S2, the aluminum alloy raw material is melted in a machine-side furnace, and the melt temperature is maintained at 700-750°C.

[0013] Preferably, the smelted aluminum alloy solution in step S2 is injected into a pulping machine, which includes a water cooling system and a heating system to keep the temperature in the pulping machine at 300-350° C. to obtain a semi-solid aluminum alloy slurry.

[0014] Preferably, in step S5, the first stage advancing speed is 0.5-1 m / s, and the shot pressure is set to 25-30 MPa, so that the aluminum alloy slurry passes through the gate slowly and steadily, ensuring that the aluminum alloy slurry passes through the gate continuously;

[0015] Preferably, in step S5, when the pushing stroke is half completed, the second stage is entered, the pushing speed of the second stage is 2-3 m / s, and the injection pressure is set to 40-50 MPa, so that the aluminum alloy slurry is quickly filled into the mold cavity;

[0016] Preferably: in step S5, when three quarters of the advancement stroke is completed, the third stage is entered, the advancement speed of the third stage is 0.2-0.6 m / s, and the shot pressure is set to 20-25 MPa for convenient pressurization treatment. After the casting is formed, the pressure is continued to be maintained at 100-150 MPa, and the maintenance time is set to 10-15 seconds.

[0017] Technical effects and advantages of the present invention:

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. Compared with the traditional direct liquid metal die casting, the shell structure die casting method of the present invention has a short solidification time and a low processing temperature, which not only improves the dimensional accuracy of the filter cavity, but also improves the productivity of the product. The shell structure die casting method of the present invention has a high forming rate, which can greatly reduce the subsequent blank processing process, reduce processing costs, and reduce energy consumption. DETAILED DESCRIPTION

[0020] The present invention will be further described in detail below in conjunction with specific embodiments. The embodiments of the present invention are provided for the purpose of illustration and description, and are not intended to be exhaustive or to limit the present invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described to better illustrate the principles and practical applications of the present invention, and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.

[0021] Example 1

[0022] In order to solve the above technical problem, the present invention provides a shell structure die-casting method in this embodiment, which includes the following steps.

[0023] S1: Customize the casting mold and process the corresponding casting mold according to the structural design of the shell;

[0024] S2: preparing metal raw materials, taking aluminum alloy raw materials and putting them into a machine-side furnace for smelting, and putting the molten metal into a pulping machine after smelting to obtain semi-solid aluminum alloy slurry;

[0025] S3: preheating the mold to 250°C;

[0026] S4: spraying a release agent onto the surfaces of the concave and convex molds of the preheated mold, and then closing the mold;

[0027] S5: Use a quantitative pump to deliver the prepared semi-solid metal into the die-casting machine, and squeeze the die-casting machine punch to push the semi-solid metal into the mold; the pushing is divided into three stages. In the first stage, the pushing is carried out at a low speed so that the aluminum alloy slurry slowly passes through the inner gate; in the second stage, the pushing speed is increased so that the aluminum alloy slurry is quickly filled into the mold cavity; in the third stage, the pushing speed is reduced so that the aluminum alloy slurry is fully filled into the mold cavity, and the casting is completed in combination with the pressurization treatment to obtain the casting blank;

[0028] S6: Heat treatment: heat-treating the above casting blank to obtain a casting product.

[0029] In step S2, the aluminum alloy raw material is melted in a machine-side furnace, and the melt temperature is maintained at 700°C.

[0030] In step S2, the smelted aluminum alloy solution is injected into a pulping machine, which includes a water cooling system and a heating system to keep the temperature in the pulping machine at 300° C. to obtain a semi-solid aluminum alloy slurry.

[0031] In step S5, the first stage advancement speed is 0.5 m / s, and the shot pressure is set to 25 MPa, so that the aluminum alloy slurry passes through the gate slowly and steadily, ensuring that the aluminum alloy slurry passes through the gate continuously; in step S5, when the advancement stroke is half completed, the second stage is entered, the advancement speed of the second stage is 2 m / s, and the shot pressure is set to 40 MPa, so that the aluminum alloy slurry is quickly filled into the mold cavity; in step S5, when the advancement stroke is three quarters completed, the third stage is entered, the advancement speed of the third stage is 0.2 m / s, and the shot pressure is set to 20 MPa, which is convenient for pressurization treatment. After casting, the pressure is continued to be maintained at 100 MPa, and the maintenance time is set to 10 seconds.

[0032] Compared with the traditional liquid metal direct die casting, the solidification time is short and the processing temperature is low, which not only improves the dimensional accuracy of the filter cavity, but also improves the productivity of the product. The shell structure die casting method of the present invention has a high forming rate, which can greatly reduce the subsequent blank processing process, reduce processing costs, and reduce energy consumption.

[0033] Example 2

[0034] In order to solve the above technical problem, the present invention provides a shell structure die-casting method in this embodiment, which includes the following steps.

[0035] S1: Customize the casting mold and process the corresponding casting mold according to the structural design of the shell;

[0036] S2: preparing metal raw materials, taking aluminum alloy raw materials and putting them into a machine-side furnace for smelting, and putting the molten metal into a pulping machine after smelting to obtain semi-solid aluminum alloy slurry;

[0037] S3: preheating the mold to 350°C;

[0038] S4: spraying a release agent onto the surfaces of the concave and convex molds of the preheated mold, and then closing the mold;

[0039] S5: Use a quantitative pump to deliver the prepared semi-solid metal into the die-casting machine, and squeeze the die-casting machine punch to push the semi-solid metal into the mold; the pushing is divided into three stages. In the first stage, the pushing is carried out at a low speed so that the aluminum alloy slurry slowly passes through the inner gate; in the second stage, the pushing speed is increased so that the aluminum alloy slurry is quickly filled into the mold cavity; in the third stage, the pushing speed is reduced so that the aluminum alloy slurry is fully filled into the mold cavity, and the casting is completed in combination with the pressurization treatment to obtain the casting blank;

[0040] S6: Heat treatment: heat-treating the above casting blank to obtain a casting product.

[0041] In step S2, the aluminum alloy raw material is melted in a machine-side furnace, and the melt temperature is maintained at 750°C.

[0042] In step S2, the smelted aluminum alloy solution is injected into a pulping machine, which includes a water cooling system and a heating system to keep the temperature in the pulping machine at 350° C. to obtain a semi-solid aluminum alloy slurry.

[0043] In step S5, the first stage advancing speed is 1m / s, and the shot pressure is set to 30 MPa, so that the aluminum alloy slurry passes through the gate slowly and steadily, ensuring that the aluminum alloy slurry passes through the gate continuously; in step S5, when the advancing stroke is half completed, the second stage is entered, the advancing speed of the second stage is 3m / s, and the shot pressure is set to 50 MPa, so that the aluminum alloy slurry is quickly filled into the mold cavity; in step S5, when the advancing stroke is three-quarters completed, the third stage is entered, the advancing speed of the third stage is 0.6m / s, and the shot pressure is set to 25 MPa, which is convenient for pressurization treatment. After casting, the pressure continues to be maintained at 150 MPa, and the maintenance time is set to 10 to 15 seconds.

[0044] Compared with the traditional liquid metal direct die casting, the solidification time is short and the processing temperature is low, which not only improves the dimensional accuracy of the filter cavity, but also improves the productivity of the product. The shell structure die casting method of the present invention has a high forming rate, which can greatly reduce the subsequent blank processing process, reduce processing costs, and reduce energy consumption.

[0045] Example 3

[0046] In order to solve the above technical problem, the present invention provides a shell structure die-casting method in this embodiment, which includes the following steps.

[0047] S1: Customize the casting mold and process the corresponding casting mold according to the structural design of the shell;

[0048] S2: preparing metal raw materials, taking aluminum alloy raw materials and putting them into a machine-side furnace for smelting, and putting the molten metal into a pulping machine after smelting to obtain semi-solid aluminum alloy slurry;

[0049] S3: preheating the mold to 300°C;

[0050] S4: spraying a release agent onto the surfaces of the concave and convex molds of the preheated mold, and then closing the mold;

[0051] S5: Use a quantitative pump to deliver the prepared semi-solid metal into the die-casting machine, and squeeze the die-casting machine punch to push the semi-solid metal into the mold; the pushing is divided into three stages. In the first stage, the pushing is carried out at a low speed so that the aluminum alloy slurry slowly passes through the inner gate; in the second stage, the pushing speed is increased so that the aluminum alloy slurry is quickly filled into the mold cavity; in the third stage, the pushing speed is reduced so that the aluminum alloy slurry is fully filled into the mold cavity, and the casting is completed in combination with the pressurization treatment to obtain the casting blank;

[0052] S6: Heat treatment: heat-treating the above casting blank to obtain a casting product.

[0053] In step S2, the aluminum alloy raw material is melted in a machine-side furnace, and the melt temperature is maintained at 730°C.

[0054] In step S2, the smelted aluminum alloy solution is injected into a pulping machine, which includes a water cooling system and a heating system to keep the temperature in the pulping machine at 320° C. to obtain a semi-solid aluminum alloy slurry.

[0055] In step S5, the first stage advancement speed is 0.8 m / s, and the shot pressure is set to 28 MPa, so that the aluminum alloy slurry passes through the gate slowly and steadily, ensuring that the aluminum alloy slurry passes through the gate continuously; in step S5, when the advancement stroke is half completed, the second stage is entered, the advancement speed of the second stage is 2.5 m / s, and the shot pressure is set to 45 MPa, so that the aluminum alloy slurry is quickly filled into the mold cavity; in step S5, when the advancement stroke is three quarters completed, the third stage is entered, the advancement speed of the third stage is 0.4 m / s, and the shot pressure is set to 23 MPa, which is convenient for pressurization treatment. After casting, the pressure is continued to be maintained at 130 MPa, and the maintenance time is set to 13 seconds.

[0056] Compared with the traditional liquid metal direct die casting, the solidification time is short and the processing temperature is low, which not only improves the dimensional accuracy of the filter cavity, but also improves the productivity of the product. The shell structure die casting method of the present invention has a high forming rate, which can greatly reduce the subsequent blank processing process, reduce processing costs, and reduce energy consumption.

[0057] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field and related fields without creative work should fall within the scope of protection of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention are implemented according to the conventional means in the field unless otherwise specified and limited.

Claims

1. A die-casting method for a housing structure, characterized in that: The following steps are included. S1: Customize the casting mold and process the corresponding casting mold according to the structural design of the shell; S2: preparing metal raw materials, taking aluminum alloy raw materials and putting them into a machine-side furnace for smelting, and putting the molten metal into a pulping machine after smelting to obtain semi-solid aluminum alloy slurry; S3: preheating the mold to 250-350°C; S4: spraying a release agent onto the surfaces of the concave and convex molds of the preheated mold, and then closing the mold; S5: Use a quantitative pump to deliver the prepared semi-solid metal into the die-casting machine, and squeeze the die-casting machine punch to push the semi-solid metal into the mold; the pushing is divided into three stages. In the first stage, the pushing is carried out at a low speed so that the aluminum alloy slurry slowly passes through the inner gate; in the second stage, the pushing speed is increased so that the aluminum alloy slurry is quickly filled into the mold cavity; in the third stage, the pushing speed is reduced so that the aluminum alloy slurry is fully filled into the mold cavity, and the casting is completed in combination with the pressurization treatment to obtain the casting blank; S6: Heat treatment: heat-treating the above casting blank to obtain a casting product.

2. A shell structure die-casting method according to claim 1, characterized in that: In step S2, the aluminum alloy raw material is melted in a machine-side furnace, and the melt temperature is maintained at 700-750°C.

3. The housing structure die-casting method according to claim 1, characterized in that: In step S2, the smelted aluminum alloy solution is injected into a pulping machine, which includes a water cooling system and a heating system to keep the temperature in the pulping machine at 300-350° C. to obtain a semi-solid aluminum alloy slurry.

4. The housing structure die-casting method according to claim 1, characterized in that: In step S5, the first stage advancement speed is 0.5-1 m / s, and the shot pressure is set to 25-30 MPa, so that the aluminum alloy slurry passes through the gate slowly and steadily, ensuring that the aluminum alloy slurry passes through the gate continuously.

5. The housing structure die-casting method according to claim 1, characterized in that: When the pushing stroke is half completed in step S5, the second stage is entered. The pushing speed of the second stage is 2-3 m / s, and the injection pressure is set to 40-50 MPa, so that the aluminum alloy slurry can be quickly filled into the mold cavity.

6. The housing structure die-casting method according to claim 1, characterized in that: In step S5, when three quarters of the advancement stroke is completed, the third stage is entered. The advancement speed of the third stage is 0.2-0.6 m / s, and the shot pressure is set to 20-25 MPa for easy pressurization treatment. After casting, the pressure is maintained at 100-150 MPa for 10-15 seconds.