Wear-resistant material for shield cutter, brazing method and automatic brazing production line
Through the combination of automatic brazing production lines and wear-resistant materials, the use of brazing methods and gradient cooling technology has solved the problems of low production efficiency of shield knives and easy deformation and oxidation of the wear-resistant layer, and improved the wear resistance and use of shield knives. life.
Patent Information
- Application Number
- CN202411031426.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
AI Technical Summary
The production efficiency of existing shield knives is low, mainly due to the slow manual welding speed, which causes thermal stress during the surfacing process of the wear-resistant layer to cause deformation and oxidation, which affects the wear-resistant effect and shortens the service life.
Using an automatic brazing production line and wear-resistant materials, the wear-resistant materials are combined with the tool base through brazing, gradient cooling technology is used to avoid thermal stress, and SiO2 nanogel film and active diamond are combined to improve wear resistance.
It improves the production efficiency and wear resistance of the shield knife, extends its service life, enhances the high-temperature oxidation resistance of the cemented carbide, and avoids deformation and oxidation of the wear-resistant layer.
Smart Images

Figure CN118768668A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding, and in particular to a wear-resistant material for a shield cutter, a brazing method and an automatic brazing production line. Background Art
[0002] Shield cutters are "the sharp teeth of a national weapon" and are highly consumable during use. Two types of failure are prone to occur during the excavation process: (1) the working surface of the carbide block is squeezed and scraped, resulting in severe wear; (2) under the action of impact and shear force, when the impact force exceeds the strength limit that the alloy material can withstand, it will cause the alloy block to crack; when the shear force exceeds the welding strength limit, it will cause the alloy block to fall off or even break the cutter.
[0003] In order to extend the service life of shield cutters, existing shield cutters are usually composed of alloy steel matrix, cemented carbide and wear-resistant layer. Among them, the alloy steel matrix mainly provides good impact toughness and protects the cemented carbide block; the cemented carbide block plays a role in directly cutting the rock and soil of the tunnel face due to its high hardness, good strength and good wear resistance; the wear resistance of the cutter is mainly achieved by surfacing a wear-resistant layer on the surface of the alloy steel matrix to prevent damage caused by wear during service.
[0004] Currently, the main domestic shield cutter manufacturers generally use manual brazing methods for preparation. The preparation process is mainly divided into two steps: the first step is to weld the wear-resistant layer to the surface of the tool steel matrix by surfacing welding to achieve wear-resistant effect; the second step is to braze the cemented carbide to the shield cutter steel matrix by using alloy welding sheets.
[0005] There is at least one of the following problems in the related technology: the shield cutter in the prior art mainly uses manual welding to weld a wear-resistant layer to the surface of the tool body to prevent damage to the shield cutter due to wear during use, but the welding process is divided into multiple steps and the manual welding speed is slow, resulting in low production efficiency of the shield cutter. Summary of the invention
[0006] The technical problem solved by the present invention is that the shield cutter in the prior art mainly uses manual welding to build up a wear-resistant layer on the surface of the cutter body to prevent damage to the shield cutter due to wear during use, but the speed of manual welding is slow, resulting in low production efficiency of the shield cutter.
[0007] To solve the above problems, a first object of the present invention is to provide a brazing method for shield cutters.
[0008] A second object of the present invention is to provide a wear-resistant material for a shield cutter.
[0009] The third object of the present invention is to provide an automatic brazing production line for shield cutters.
[0010] To achieve the above-mentioned first purpose, the present invention provides a brazing method for a shield blade, the brazing method is used to prepare a shield blade, and the brazing method is applied to an automatic brazing production line, the automatic brazing production line includes a preheating furnace, a transition chamber, a welding chamber, and a first paste dispenser, and the brazing method includes: S100: Assembling the alloy steel matrix and the cemented carbide to obtain a tool matrix, placing the tool matrix on a loading rack, and conveying the tool matrix to a preheating furnace by the loading rack for preheating treatment; S200: sending the tool substrate that has completed the preheating treatment into a transition chamber for at least one gas washing operation; S300: Pushing the tool substrate after the gas washing operation into the welding chamber, and performing the first coating operation on the cemented carbide by the first paste dispenser; S400: performing a brazing operation on the tool substrate that has completed the first coating operation to obtain a shield tool.
[0011] Compared with the existing technology, the technical effect achieved by adopting this technical solution is as follows: in the manufacturing process of the shield cutter, the brazing method is used to realize the demand for automated production, avoiding the slow speed of manual welding, which leads to low production efficiency of the shield cutter, thereby improving the production efficiency of the shield cutter.
[0012] Specifically, in the prior art, a wear-resistant layer is welded to the surface of the tool body by manual welding to prevent the shield cutter from being damaged by wear during use. During manual operation, the entire production cycle of the shield cutter is prolonged due to the slow speed of manual operation, thereby affecting the production efficiency of the shield cutter. This solution provides a brazing method, which is applied to an automatic brazing production line. An automatic welding method is used to replace the manual welding method. Automatic welding can increase the welding speed, reduce human errors, and improve production efficiency.
[0013] In one embodiment of the present invention, the automatic brazing production line further includes a heat preservation furnace and a second paste dispenser, and S400 specifically includes: S410: The second paste dispensing machine performs a second coating operation on the working surface of the tool base; S420: performing a wear-resistant brazing operation on the working surface after the second coating operation; S430: sending the tool substrate that has completed the wear-resistant brazing action into a heat preservation furnace for gradient cooling.
[0014] Compared with the prior art, the technical effect achieved by adopting this technical solution is: the wear resistance of the shield cutter is improved, thereby ensuring the service life of the shield cutter.
[0015] Specifically, the shield cutter in the prior art mainly combines the wear-resistant layer with the cutter body by surfacing welding to prevent damage to the shield cutter due to wear during use. However, due to the rapid heating and cooling during the surfacing welding process, thermal stress is generated in the wear-resistant area, causing deformation and cracks in the wear-resistant layer, which makes the wear-resistant layer at the cracks easily oxidized, thereby affecting the wear-resistant effect of the wear-resistant layer.
[0016] Furthermore, the present solution forms a wear-resistant layer by coating the wear-resistant material on the shield cutter, combining the wear-resistant material with the cutter substrate by wear-resistant brazing, and then reducing the temperature of the shield cutter to room temperature by gradient cooling, thereby avoiding thermal stress in the wear-resistant area, which may cause deformation and cracks in the wear-resistant layer and oxidation of the wear-resistant layer, thereby improving the wear-resistant effect of the wear-resistant layer and extending the service life of the shield cutter.
[0017] In one embodiment of the present invention, S300 specifically includes: S310: mixing a first silane coupling agent and water to react once to obtain a coating material, and loading the coating material into a first paste dispensing machine (300); The S400 also includes: S440: preparing a wear-resistant material, and loading the wear-resistant material into the second paste dispensing machine (400).
[0018] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: improving the wear resistance of the shield cutter and enhancing the high-temperature oxidation resistance of the cemented carbide.
[0019] Specifically, the first silane coupling agent is mixed with water to undergo a hydrolysis reaction to generate a coating material carrying a silanol group (-Si—OH), and then the coating material is applied to the surface of the cemented carbide by a second paste dispenser. Cemented carbide is an inorganic substance with a certain amount of hydroxyl groups (-OH) on the surface. The hydroxyl groups (-OH) react with the silanol groups (-Si—OH) of the coating material to form a dense SiO layer on the surface of the cemented carbide. 2 Nanogel film, SiO 2 The nanogel film can rely on its own cross-linking shrinkage stress to continuously and densely coat the surface of the cemented carbide, isolate the air on the surface of the cemented carbide to form a protective layer, thereby improving the high-temperature oxidation resistance of the cemented carbide.
[0020] In one embodiment of the present invention, the temperature of the primary reaction is 20° C. to 60° C.; and / or the pressure of the primary reaction is 7 MPa to 9 MPa; and / or the time of the primary reaction is 30 min to 50 min.
[0021] Compared with the prior art, the technical effect achieved by adopting this technical solution is: improving the conversion rate of a primary reaction and improving the utilization rate of materials.
[0022] Specifically, the first silane coupling agent and water are mixed to undergo a hydrolysis reaction to generate an intermediate product carrying a silanol group (-Si—OH). The temperature of the primary reaction is controlled at 20°C to 60°C to accelerate the chemical reaction rate, thereby increasing the conversion rate of the primary reaction and allowing the silane coupling agent to be fully hydrolyzed. Furthermore, the present invention preferably sets the primary reaction time to 30 minutes, accurately controls the reaction time of the hydrolysis of the silane coupling agent, avoids unnecessary side reactions, thereby further increasing the conversion rate of the silane coupling agent and improving the utilization rate of the material. The pressure during the primary reaction is controlled at 7MPa to 9MPa to increase the concentration of the reactants, thereby further accelerating the reaction rate of the primary reaction.
[0023] In an example of the present invention, S440 specifically includes: S441: mixing the second silane coupling agent and water for a secondary reaction to obtain an intermediate product; S442: mixing the intermediate product with carboxyl boronic acid and catalyst A to react three times to obtain an activation solution; S443: mixing the activation liquid with diamond, heating, and screening to obtain active diamond; S444: adding a solvent, a soldering flux, and a thixotropic agent into a reaction kettle, mixing and stirring, to obtain a soldering flux paste; S445: Active diamond, silver-based solder and flux paste are mixed and stirred to obtain wear-resistant material.
[0024] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: this solution improves the wear resistance of the wear-resistant material by adding active diamond into the silver-based solder as the hard phase of the wear-resistant material.
[0025] Specifically, diamond is composed of carbon atoms tightly arranged in a tetrahedral structure, and each carbon atom is connected to the surrounding carbon atoms through strong and stable covalent bonds. Therefore, diamond has relatively stable chemical properties. However, when the temperature of traditional diamond exceeds 700°C, diamond is easy to carbonize, which reduces the physical properties of diamond and further affects the wear resistance of diamond. This scheme activates diamond by preparing an activation liquid to protect diamond from carbonization in an environment exceeding 700°C. At the same time, diamond has its own active groups to enhance the bonding force between diamond and metal and improve the connection activity and strength of diamond.
[0026] Furthermore, the intermediate product reacts with carboxyl boric acid under the action of catalyst A to generate an activation solution carrying both boric acid groups and silanol groups (-Si—OH). After the activation solution is mixed with diamond, the silanol groups (-Si—OH) of the activation solution react with the active hydroxyl groups on the surface of the diamond to form hydrogen bonds and condense into -SiO—M covalent bonds (M represents the surface of the diamond particles), making them adsorbed and connected. At the same time, the condensation reaction proceeds in a multi-dimensional direction, and the silanol groups (-Si—OH) of each silane molecule associate and aggregate with each other to form a three-dimensional short-chain cross-linked network structure of gel aggregates (SiO 2 The cross-linked polymer film is covered on the surface of the diamond powder particles to make the diamond surface organic and functional. Then SiO containing active oxygen groups is obtained on the diamond surface. 2 Nanogel film can be coated on the surface of diamond particles continuously and densely by its own cross-linking shrinkage stress, which can evenly disperse diamonds and make the hard phase in the wear-resistant material evenly distributed, avoiding the diamond agglomeration that is easy to occur in traditional preparation methods; at the same time, it can isolate the air on the surface of diamond to form a protective layer, improving the high-temperature oxidation resistance of diamond. The boric acid active group carried by silane is adsorbed on the surface of diamond along with silane, and the boric acid (H 3 BO 3 ) decomposes into boron hepatite (B 2 O 3 ), the boron liver (B 2 O 3 ) forms fusible borates with metal oxides, thereby enhancing the ability to remove interface oxides, and further enhancing the connection strength between diamond and silver-based solder, making it difficult for diamond to fall off and enhancing the adhesion between the wear-resistant material and the diamond surface.
[0027] In one embodiment of the present invention, the temperature of the secondary reaction is 40°C to 90°C; and / or the pressure of the secondary reaction is 7MPa to 9MPa; and / or the time of the secondary reaction is 25min to 35min; and / or the temperature of the tertiary reaction is 60°C to 70°C; and / or the time of the tertiary reaction is 1h to 1.5h; and / or the time of mixing the activation solution with the diamond and heating is 3h to 3.5h; and / or the temperature of mixing the activation solution with the diamond and heating is 60°C to 80℃; and / or the temperature for adding the solvent, flux and thixotropic agent into the reaction kettle for mixing and stirring is 90℃~150℃; and / or the temperature for mixing and stirring the active diamond, silver-based solder and solder paste is 15℃~30℃; and / or the time for mixing and stirring the active diamond, silver-based solder and solder paste is 1.5h~2.5h; and / or the vacuum degree for mixing and stirring the active diamond, silver-based solder and solder paste is -80KPa~-100KPa.
[0028] Compared with the prior art, the technical effect achieved by adopting this technical solution is: improving the oxidation resistance of diamond and enhancing the surface activation performance of diamond.
[0029] Specifically, the silane coupling agent and water are mixed to undergo a hydrolysis reaction to generate a coating material carrying a silanol group (-Si—OH). The temperature of the secondary reaction is controlled to be 40°C-90°C to accelerate the speed of the chemical reaction, thereby increasing the conversion rate of the secondary reaction and allowing the silane coupling agent to be fully hydrolyzed. Furthermore, the preferred secondary reaction time of the present invention is 30 minutes, and the reaction time of the hydrolysis of the silane coupling agent is accurately controlled to avoid unnecessary side reactions, thereby further increasing the conversion rate of the silane coupling agent and improving the utilization rate of the material. The pressure during the secondary reaction is controlled to increase the concentration of the reactants, thereby further accelerating the reaction rate of the secondary reaction.
[0030] Furthermore, the temperature of the three reactions is controlled to be 60° C. to 70° C., the time of the three reactions is controlled to be 1 h to 1.5 h, and preferably the time of the three reactions is 1 h, so that during the three reactions, the intermediate product, the carboxyl boric acid and the catalyst A can be evenly mixed, thereby improving the conversion rate of the three reactions and the utilization rate of the materials.
[0031] Preferably, the active diamond, silver-based solder and flux paste are mixed and stirred for 2 hours, and the vacuum degree for mixing and stirring the active diamond, silver-based solder and flux paste is -90KPa, so as to further improve the wear resistance of the wear-resistant material and thereby extend the service life of the shield cutter.
[0032] To achieve the second purpose of the present invention, the present invention also provides a wear-resistant material for a shield cutter, the wear-resistant material is used in the brazing method described in any of the above technical solutions, the wear-resistant material includes 2 to 8 parts by mass of active diamond micropowder; 4 to 10 parts by mass of active nanodiamond; 2 to 6 parts by mass of solvent; 1 to 3 parts by mass of thixotropic agent; 1 to 5 parts by mass of flux; 81 to 93 parts by mass of silver-based solder; wherein the silver-based solder is selected from at least one of Ag43CuZnNi, Ag40CuZnNiMn, Ag33CuZnSnNiMn, and Ag28CuZnNiMn.
[0033] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant material is improved, thereby extending the service life of the shield cutter.
[0034] Specifically, the wear-resistant material includes composite diamond particles composed of diamond micropowder and nanodiamonds, which increases the diamond content on the wear surface of the wear-resistant layer, and the exposure of nanodiamonds fills the gaps in the diamond micropowder, protecting the silver-based solder alloy matrix. Furthermore, after adding nanodiamonds, the diamonds on the coating surface tend to be saturated, increasing the proportion of diamonds per unit area, improving the wear resistance of the shield cutter, and thus extending the service life of the shield cutter.
[0035] In one embodiment of the present invention, the silver-based solder is a powder material, and the particle size of the powder material is 200-300 mesh; and / or the particle size of the active diamond micropowder is 30 μm-60 μm; and / or the particle size of the active nanodiamond is 100 nm-200 nm.
[0036] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant material is further improved, thereby extending the service life of the shield cutter.
[0037] In one embodiment of the present invention, the solvent is selected from one or more of glycerol, fatty alcohol, and octanol; and / or the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax; and / or the flux is selected from one or more of borax and potassium fluoride.
[0038] Compared with the prior art, the technical effect achieved by adopting the technical scheme is as follows: borax and potassium fluoride are selected as flux to remove oxides on the welding surface, thereby promoting the bonding between diamond and metal; the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax, and the solvent is selected from one or more of propylene glycol, fatty alcohol, and octanol to prevent the sedimentation of diamond and metal powder, thereby avoiding the liquid-solid separation phenomenon of the wear-resistant material.
[0039] To achieve the third purpose of the present invention, the present invention also provides an automatic brazing production line for shield cutters. The automatic brazing production line adopts the brazing method described in any of the above technical solutions. The automatic brazing production line includes a preheating furnace, which is used to preheat the tool substrate placed on the loading rack; a transition chamber, which is connected to the preheating furnace and is used to perform at least one gas washing operation on the tool substrate that has completed the preheating treatment; a first paste dispensing machine, which is used to perform a first coating action on the cemented carbide; a second paste dispensing machine, which is used to perform a second coating action on the working surface of the tool substrate; a welding chamber, which is arranged at one end of the transition chamber away from the preheating furnace, and is used to perform a brazing action on the tool substrate that has completed the first coating action; and an insulation furnace, which is arranged at one end of the welding chamber away from the transition chamber, and is used to perform a gradient cooling on the shield cutter that has completed the brazing action.
[0040] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: the automatic brazing production line is adopted to realize the demand for automated production, avoiding the slow speed of manual welding, which leads to low production efficiency of the shield cutter, thereby improving the production efficiency of the shield cutter.
[0041] Preferably, the welding chamber further comprises a positioner and an induction coil, wherein the positioner is used to lift the alloy steel substrate that has completed the second coating action and the hard alloy that has completed the first coating action to the position where the induction coil is located; Preferably, the welding chamber further comprises an induction power supply and a welding position, the induction power supply is in communication connection with the induction coil, and the induction coil is driven by the induction power supply to adjust the alloy steel substrate that has completed the second coating action and the hard alloy that has completed the first coating action to the welding position; after the induction power supply is turned on, the welding chamber performs a brazing action on the alloy steel substrate that has completed the second coating action and the hard alloy that has completed the first coating action; Preferably, the welding chamber also includes a conveyor chain plate for carrying the shield cutter that has completed gradient cooling out of the insulation furnace.
[0042] After adopting the technical solution of the present invention, the following technical effects can be achieved: (1) The present invention provides a wear-resistant material, a brazing method and an automatic brazing production line for shield cutters. In the manufacturing process of shield cutters, the brazing method provided by the present invention is used to meet the needs of automated production, avoid the situation where the production efficiency of shield cutters is low due to the slow speed of manual welding, and thus improve the production efficiency of shield cutters; (2) The present invention provides a wear-resistant material, a brazing method and an automatic brazing production line for a shield cutter, thereby improving the wear resistance of the wear-resistant material and thereby extending the service life of the shield cutter; (3) The present invention provides a wear-resistant material, a brazing method and an automatic brazing production line for shield cutters. The automatic brazing production line is adopted to meet the demand for automated production, avoid the situation where the slow speed of manual welding leads to low production efficiency of shield cutters, thereby improving the production efficiency of shield cutters; (4) The present invention provides a wear-resistant material, a brazing method and an automatic brazing production line for shield cutters. The automatic brazing production line is used to apply a coating material on the surface of the cemented carbide. The coating material forms a dense SiO2 nanogel film on the surface of the cemented carbide. The SiO2 nanogel film can rely on its own cross-linking shrinkage stress to continuously and densely coat the surface of the cemented carbide, isolate the air on the surface of the cemented carbide to form a protective layer, thereby improving the high-temperature oxidation resistance of the cemented carbide. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings to be used in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work. Figure 1 Reaction formula 1 provided in an embodiment of the present invention; Figure 2 Reaction formula 2 provided in an embodiment of the present invention; Figure 3 Reaction formula 3 provided in an embodiment of the present invention; Figure 4 Reaction formula 4 provided in an embodiment of the present invention; Figure 5 Reaction formula 5 provided in an embodiment of the present invention; Figure 6 A schematic diagram of the structure of an automatic brazing production line provided by an embodiment of the present invention; Figure 7 for Figure 6 Enlarged view of area A in the middle; Figure 8 This is a mirror image of the wear-resistant layer provided in Comparative Example 1 of the present invention; Fig. 9 A mirror image of the wear-resistant layer provided in Example 1 of the present invention; Fig.10 This is a mirror image of the cemented carbide after being coated with a coating material provided by an embodiment of the present invention.
[0044] Description of reference numerals: 100, preheating furnace; 200, transition chamber; 300, first paste dispensing machine; 310, first feeding pipe; 400, second paste dispensing machine; 410, second feeding pipe; 500, welding chamber; 600, holding furnace. DETAILED DESCRIPTION
[0045] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0046] The present invention provides a brazing method for a shield blade, the brazing method is used to prepare a shield blade, the brazing method is applied to an automatic brazing production line, the automatic brazing production line includes a preheating furnace 100, a transition chamber 200, a welding chamber 500, and a first paste dispenser 300, and the brazing method includes: S100: placing the alloy steel matrix and cemented carbide for assembling the shield blade on a loading rack, and the loading rack transports the alloy steel matrix and cemented carbide to a preheating furnace 100 for preheating treatment; S200: sending the alloy steel substrate and cemented carbide that have completed the preheating treatment into the transition chamber 200 to perform at least one gas washing operation; S300: Pushing the alloy steel substrate and the cemented carbide after the gas washing operation into the welding chamber 500, and performing the first coating operation on the surface of the cemented carbide by the first paste dispenser 300; S400: performing a brazing operation on the alloy steel substrate that has completed the preheating treatment and the cemented carbide that has completed the first coating operation to obtain a shield blade.
[0047] This solution uses a brazing method in the manufacturing process of the shield cutter, which realizes the demand for automated production and avoids the situation where the slow speed of manual welding leads to low production efficiency of the shield cutter, thereby improving the production efficiency of the shield cutter.
[0048] Specifically, in the prior art, a wear-resistant layer is welded to the surface of the tool body by manual welding to prevent the shield cutter from being damaged by wear during use. During manual operation, the entire production cycle of the shield cutter is prolonged due to the slow speed of manual operation, thereby affecting the production efficiency of the shield cutter. This solution provides a brazing method, which is applied to an automatic brazing production line. An automatic welding method is used to replace the manual welding method. Automatic welding can increase the welding speed, reduce human errors, and improve production efficiency.
[0049] Furthermore, the automatic brazing production line further includes a heat preservation furnace 600 and a second paste dispenser 400, and S400 specifically includes: S410: The second paste dispensing machine 400 performs a second coating operation on the working surface of the tool base; S420: performing a wear-resistant brazing operation on the working surface after the second coating operation; S430: sending the tool substrate that has completed the wear-resistant brazing operation into the insulation furnace 600 for gradient cooling.
[0050] This solution improves the wear resistance of the shield cutter, thereby ensuring the service life of the shield cutter.
[0051] Specifically, the shield cutter in the prior art mainly combines the wear-resistant layer with the cutter body by surfacing welding to prevent damage to the shield cutter due to wear during use. However, due to the rapid heating and cooling during the surfacing welding process, thermal stress is generated in the wear-resistant area, causing deformation and cracks in the wear-resistant layer, which makes the wear-resistant layer at the cracks easily oxidized, thereby affecting the wear-resistant effect of the wear-resistant layer.
[0052] Specifically, this solution forms a wear-resistant layer by coating the wear-resistant material on the shield cutter, combining the wear-resistant material with the cutter base through wear-resistant brazing, and then reducing the temperature of the shield cutter to room temperature through gradient cooling. This avoids thermal stress in the wear-resistant area, which may cause deformation and cracks in the wear-resistant layer and oxidation of the wear-resistant layer, thereby improving the wear resistance of the wear-resistant layer and extending the service life of the shield cutter.
[0053] Furthermore, S300 specifically includes: S310: mixing a first silane coupling agent and water to react once to obtain a coating material, and loading the coating material into a first paste dispensing machine (300); The S400 also includes: S440: preparing a wear-resistant material, and loading the wear-resistant material into the second paste dispensing machine (400).
[0054] Thereby improving the wear resistance of the shield cutter and enhancing the high temperature oxidation resistance of the cemented carbide.
[0055] For example, if Figure 1 and Figure 2 As shown, the first silane coupling agent of the embodiment of the present invention is trimethoxysilane. After the trimethoxysilane is mixed with water, a hydrolysis reaction occurs to generate a coating material carrying a silanol group (-Si—OH). The coating material is then coated on the surface of the cemented carbide by the first paste dispenser 300. The cemented carbide is an inorganic substance, and there are certain hydroxyl groups (-OH) on the surface. The hydroxyl groups (-OH) react with the silanol groups (-Si—OH) of the coating material to form a dense SiO layer on the surface of the cemented carbide. 2 Nanogel film, SiO 2 The nanogel film can rely on its own cross-linking shrinkage stress to continuously and densely coat the surface of the cemented carbide, isolate the air on the surface of the cemented carbide to form a protective layer, thereby improving the high-temperature oxidation resistance of the cemented carbide.
[0056] Preferably, the general formula of the first silane coupling agent is R—Si—X3, wherein R is an organic functional group that can react or act with the polymer material, such as methyl, vinyl, octenyl, amino, etc.; X is a hydrolyzable group, and Si—X forms silanol Si—OH after hydrolysis.
[0057] Furthermore, the temperature of the primary reaction is 20° C. to 60° C.; and / or the pressure of the primary reaction is 7 MPa to 9 MPa; and / or the time of the primary reaction is 30 min to 50 min.
[0058] This solution improves the conversion rate of a single reaction and improves the utilization rate of materials.
[0059] Specifically, the first silane coupling agent and water are mixed to undergo a hydrolysis reaction to generate an intermediate product carrying a silanol group (-Si—OH). The temperature of the primary reaction is controlled at 20°C to 60°C to accelerate the chemical reaction rate, thereby increasing the conversion rate of the primary reaction and allowing the silane coupling agent to be fully hydrolyzed. Furthermore, the present invention preferably sets the primary reaction time to 30 minutes, accurately controls the reaction time of the hydrolysis of the silane coupling agent, avoids unnecessary side reactions, thereby further increasing the conversion rate of the silane coupling agent and improving the utilization rate of the material. The pressure during the primary reaction is controlled at 7MPa to 9MPa to increase the concentration of the reactants, thereby further accelerating the reaction rate of the primary reaction.
[0060] Further, S441: mixing the second silane coupling agent and water for a secondary reaction to obtain an intermediate product; S442: mixing the intermediate product with carboxyl boronic acid and catalyst A to react three times to obtain an activation solution; S443: mixing the activation liquid with diamond, heating, and screening to obtain active diamond; S444: adding a solvent, a soldering flux, and a thixotropic agent into a reaction kettle, mixing and stirring, to obtain a soldering flux paste; S445: Active diamond, silver-based solder and flux paste are mixed and stirred to obtain wear-resistant material.
[0061] This solution improves the wear-resistant effect of the wear-resistant material by adding active diamond into the silver-based solder as the hard phase of the wear-resistant material.
[0062] Specifically, diamond is composed of carbon atoms tightly arranged in a tetrahedral structure, and each carbon atom is connected to the surrounding carbon atoms through strong and stable covalent bonds. Therefore, diamond has relatively stable chemical properties. However, when the temperature of traditional diamond exceeds 700°C, diamond is easy to carbonize, which reduces the physical properties of diamond and further affects the wear resistance of diamond. This scheme activates diamond by preparing an activation liquid to protect diamond from carbonization in an environment exceeding 700°C. At the same time, diamond has its own active groups to enhance the bonding force between diamond and metal and improve the connection activity and strength of diamond.
[0063] For example, if Figures 3 to 5As shown, the second silane coupling agent used in the embodiment of the present invention is vinyl trimethoxysilane. Vinyl trimethoxysilane and water are mixed to undergo a hydrolysis reaction. After the vinyl trimethoxysilane is hydrolyzed, an intermediate product carrying both a silanol group (-Si—OH) and ethyl alcohol is generated. The intermediate product reacts with carboxyl boric acid under the action of catalyst A to generate an activation solution carrying both a boric acid group and a silanol group (-Si—OH). After the activation solution is mixed with diamond, the silanol group (-Si—OH) of the activation solution undergoes a condensation reaction with the active hydroxyl group on the surface of the diamond to form a hydrogen bond and condense into a -SiO—M covalent bond (M represents the surface of the diamond particle), so that it is adsorbed and connected. At the same time, the condensation reaction proceeds in a multi-dimensional direction, and the silanol groups (-Si—OH) of each silane molecule associate and aggregate with each other to form a gel aggregate (SiO 2 The cross-linked polymer film is covered on the surface of the diamond powder particles to make the diamond surface organic and functional. Then SiO containing active oxygen groups is obtained on the diamond surface. 2 Nanogel film can be coated on the surface of diamond particles continuously and densely by its own cross-linking shrinkage stress, which can evenly disperse diamonds and make the hard phase in the wear-resistant material evenly distributed, avoiding the diamond agglomeration that is easy to occur in traditional preparation methods; at the same time, it can isolate the air on the surface of diamond to form a protective layer, improving the high-temperature oxidation resistance of diamond. The boric acid active group carried by silane is adsorbed on the surface of diamond along with silane, and the boric acid (H 3 BO 3 ) decomposes into boron hepatite (B 2 O 3 ), the boron liver (B 2 O 3 ) forms fusible borates with metal oxides, thereby enhancing the ability to remove interface oxides, and further enhancing the connection strength between diamond and silver-based solder, making it difficult for diamond to fall off and enhancing the adhesion between the wear-resistant material and the diamond surface.
[0064] For example, the carboxyl boronic acid provided in the embodiment of the present invention is (2,5-dicarboxyphenyl)boric acid, such as Figure 2 As shown, it is a reaction formula for the reaction of the coating material provided by an embodiment of the present invention and (2,5-dicarboxyphenyl)boric acid, wherein the hydroxyl group (-OH) of ethyl alcohol in the coating material and the carboxyl group (-COOH) of (2,5-dicarboxyphenyl)boric acid undergo an esterification reaction under the action of catalyst A to generate an activation solution carrying both a boric acid group and a silanol group (-Si—OH). After the activation solution is mixed with diamond, the silanol group (-Si—OH) of the activation solution undergoes a condensation reaction with the active hydroxyl group on the surface of the diamond to perform adsorption interconnection.
[0065] Preferably, the catalyst A of the present invention is selected from one or more of zinc oxide and stannous chloride to accelerate the esterification reaction between the hydroxyl group (-OH) of ethyl alcohol in the coating material and the carboxyl group (-COOH) of (2,5-dicarboxyphenyl)boric acid.
[0066] Furthermore, the temperature of the secondary reaction is 40°C to 90°C; and / or the pressure of the secondary reaction is 7MPa to 9MPa; and / or the time of the secondary reaction is 25min to 35min; and / or the temperature of the tertiary reaction is 60°C to 70°C; and / or the time of the tertiary reaction is 1h to 1.5h; and / or the time for mixing and heating the activation solution and diamond is 3h to 3.5h; and / or the temperature for mixing and heating the activation solution and diamond is 60°C to 80°C; and / or the temperature for adding the solvent, flux and thixotropic agent into the reaction kettle for mixing and stirring is 90°C to 150°C; and / or the temperature for mixing and stirring the active diamond, silver-based solder and solder paste is 15°C to 30°C; and / or the time for mixing and stirring the active diamond, silver-based solder and solder paste is 1.5h to 2.5h; and / or the vacuum degree for mixing and stirring the active diamond, silver-based solder and solder paste is -80KPa to -100KPa.
[0067] This solution improves the oxidation resistance of diamond and enhances the surface activation performance of diamond.
[0068] Specifically, the silane coupling agent and water are mixed to undergo a hydrolysis reaction to generate a coating material carrying a silanol group (-Si—OH). The temperature of the secondary reaction is controlled to be 40°C-90°C to accelerate the speed of the chemical reaction, thereby increasing the conversion rate of the secondary reaction and allowing the silane coupling agent to be fully hydrolyzed. Furthermore, the preferred secondary reaction time of the present invention is 30 minutes, and the reaction time of the hydrolysis of the silane coupling agent is accurately controlled to avoid unnecessary side reactions, thereby further increasing the conversion rate of the silane coupling agent and improving the utilization rate of the material. The pressure during the secondary reaction is controlled to increase the concentration of the reactants, thereby further accelerating the reaction rate of the secondary reaction.
[0069] Specifically, the temperature of the tertiary reaction is controlled to be 60° C. to 70° C., the time of the tertiary reaction is controlled to be 1 h to 1.5 h, and preferably the time of the tertiary reaction is 1 h, so that during the tertiary reaction, the intermediate product, the carboxyl boric acid and the catalyst A can be evenly mixed, thereby improving the conversion rate of the tertiary reaction and the utilization rate of the materials.
[0070] Preferably, the active diamond, silver-based solder and flux paste are mixed and stirred for 2 hours, and the vacuum degree for mixing and stirring the active diamond, silver-based solder and flux paste is -90KPa, so as to further improve the wear resistance of the wear-resistant material and thereby extend the service life of the shield cutter.
[0071] Furthermore, the present invention also provides a wear-resistant material for a shield cutter, the wear-resistant material is used in the brazing method described in any of the above technical solutions, the wear-resistant material includes 2 to 8 parts by mass of active diamond micropowder; 4 to 10 parts by mass of active nanodiamond; 2 to 6 parts by mass of solvent; 1 to 3 parts by mass of thixotropic agent; 1 to 5 parts by mass of flux; 81 to 93 parts by mass of silver-based solder; wherein the silver-based solder is selected from at least one of Ag43CuZnNi, Ag40CuZnNiMn, Ag33CuZnSnNiMn, and Ag28CuZnNiMn.
[0072] This solution improves the wear resistance of wear-resistant materials, thereby extending the service life of shield cutters.
[0073] Specifically, the wear-resistant material includes composite diamond particles composed of diamond micropowder and nanodiamonds, which increases the diamond content on the wear surface of the wear-resistant layer, and the exposure of nanodiamonds fills the gaps in the diamond micropowder, protecting the silver-based solder alloy matrix. Furthermore, after adding nanodiamonds, the diamonds on the coating surface tend to be saturated, increasing the proportion of diamonds per unit area, improving the wear resistance of the shield cutter, and thus extending the service life of the shield cutter.
[0074] Furthermore, the silver-based solder is a powder material, and the particle size of the powder material is 200-300 meshes; and / or the particle size of the active diamond micropowder is 30-60 μm; and / or the particle size of the active nanodiamond is 100-200 nm.
[0075] This solution further improves the wear resistance of the wear-resistant material, thereby extending the service life of the shield cutter.
[0076] Furthermore, the solvent is selected from one or more of glycerol, fatty alcohol, and octanol; and / or the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax; and / or the flux is selected from one or more of borax and potassium fluoride.
[0077] This scheme selects borax and potassium fluoride as flux to remove oxides on the welding surface, thereby promoting the bonding between diamond and metal; the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax, and the solvent is selected from one or more of propylene glycol, fatty alcohol, and octanol to prevent the sedimentation of diamond and metal powder, thereby avoiding the liquid-solid separation of the wear-resistant material.
[0078] Further, such as Figure 6 and Figure 7As shown, the present invention also provides an automatic brazing production line for a shield cutter. The automatic brazing production line adopts the brazing method described in any of the above technical solutions. The automatic brazing production line includes a preheating furnace 100, a transition chamber 200, a first paste dispensing machine 300, a second paste dispensing machine 400, a welding chamber 500, and an insulation furnace 600. Among them, the preheating furnace 100 includes a device for preheating the alloy steel substrate and the cemented carbide placed on the loading rack, the transition chamber 200 is connected to the preheating furnace 100, and is used to perform at least one gas washing operation on the alloy steel substrate and the cemented carbide that have completed the preheating treatment, the first paste dispensing machine 300 is used to perform a first coating action on the surface of the cemented carbide, and the second paste dispensing machine 400 is used to perform a second coating action on the surface of the alloy steel substrate, the welding chamber 500 is arranged at one end of the transition chamber 200 away from the preheating furnace 100, and is used to perform a brazing action on the alloy steel substrate that has completed the second coating action and the cemented carbide that has completed the first coating action, and the insulation furnace 600 is arranged at one end of the welding chamber 500 away from the transition chamber 200, and is used to perform a gradient cooling on the shield cutter that has completed the brazing action.
[0079] This solution adopts an automatic brazing production line to meet the needs of automated production, avoiding the situation where slow manual welding leads to low production efficiency of shield cutters, thereby improving the production efficiency of shield cutters.
[0080] Preferably, Figure 7 As shown, the welding chamber 500 is further provided with a first feeding pipe 310 connected to the first paste dispensing machine 300 , and a second feeding pipe 410 connected to the second paste dispensing machine 400 .
[0081] Preferably, the welding chamber 500 further comprises a positioner and an induction coil, wherein the positioner is used to lift the alloy steel substrate that has completed the second coating action and the cemented carbide that has completed the first coating action to the position where the induction coil is located; Preferably, the welding chamber 500 further comprises an induction power supply 700 and a welding position, wherein the induction power supply 700 is in communication connection with the induction coil, and the induction coil is driven by the induction power supply 700 to adjust the alloy steel substrate that has completed the second coating action and the cemented carbide that has completed the first coating action to the welding position; after the induction power supply 700 is turned on, the welding chamber 500 performs a brazing action on the alloy steel substrate that has completed the second coating action and the cemented carbide that has completed the first coating action; Preferably, the welding chamber 500 further includes a conveying chain plate for carrying the shield cutter that has completed the gradient cooling out of the insulation furnace 600.
[0082] Preferably, in the automatic brazing production line provided by the present invention, two transition chambers 200 are provided, and the two transition chambers 200 are respectively provided at both ends of the welding chamber 500, for performing at least one gas washing operation on the alloy steel substrate and the cemented carbide that have completed the preheating treatment, so as to prevent the oxygen content in the welding chamber 500 from being higher than a set standard value, thereby oxidizing the alloy steel substrate and the cemented carbide.
[0083] Specifically, the transition chamber 200 provided in the embodiment of the present invention uses nitrogen or argon to perform at least one gas washing operation on the alloy steel substrate and cemented carbide that have completed the preheating treatment.
[0084] [Example 1] This embodiment provides a shield cutter, and the specific operation is as follows.
[0085] Step 1: react trimethoxysilane with water at a temperature of 20° C. to 60° C. and a pressure of 7 MPa to 9 MPa for 30 minutes to generate a coating material.
[0086] Step 2: Calculate by mass, weigh 4 parts by mass of propylene glycol, 1 part by mass of polyamide wax, 2 parts by mass of borax, and 1 part by mass of potassium fluoride, put them into a reactor, stir and mix them evenly at 90°C ~ 150°C to obtain soldering paste; cool to 15°C ~ 30°C, weigh 2 parts by mass of modified active diamond micropowder and 4 parts by mass of nano-active diamond, and 89 parts by mass of Ag43CuZnNi solder powder, add them into the reactor, stir at 15°C ~ 30°C for 2 hours, and obtain a wear-resistant material.
[0087] Step three: Load the prepared coating material into the first paste dispensing machine, and use the first paste dispensing machine 300 to apply the coating material to the surface of the cemented carbide.
[0088] Step 4: Load the prepared wear-resistant material into the second paste dispensing machine 400, and use the second paste dispensing machine 400 to evenly coat the wear-resistant material on the working surface of the tool substrate, and control the thickness of the coating layer to be 5 mm, and dry it at 100° C. for 15 minutes.
[0089] Step 5: Place the tool base coated with wear-resistant material after drying on a high-temperature resistant bracket for fixation, heat it to 700℃~900℃ through induction heating, perform gradient heating for 40 minutes, stay for 3 minutes after completing the gradient heating, and then transport the shield tool to the insulation furnace 600 for gradient cooling. Finally, the conveyor chain plate will take the shield tool that has completed the gradient cooling out of the insulation furnace 600.
[0090] [Example 2] This embodiment provides a shield cutter, and its preparation method refers to that of Embodiment 1, except that, in step one, the active diamond powder is 3 parts by mass, the nano-active diamond is 5 parts by mass, and the Ag43CuZnNi solder powder is 87 parts by mass.
[0091] [Example 3] This embodiment provides a shield cutter, and its preparation method refers to that of Embodiment 1, except that, in step one, the active diamond micropowder is 4 parts by mass, the nano-active diamond is 6 parts by mass, the Ag43CuZnNi solder powder is 85 parts by mass, and the propylene glycol is 5 parts by mass.
[0092] [Example 4] This embodiment provides a shield cutter, and its preparation method refers to that of Embodiment 1, except that, in step one, the active diamond micropowder is 5 parts by mass, the nano-active diamond is 7 parts by mass, the Ag43CuZnNi solder powder is 83 parts by mass, and the propylene glycol is 5 parts by mass.
[0093] [Comparative Example 1] This comparative example provides a shield cutter, and its preparation method refers to Example 1, except that the preparation materials in step 2 are: 2 parts by mass of ordinary diamond powder (30μm~40μm), 4 parts by mass of nano diamond (100nm~150nm), 4 parts by mass of propylene glycol, 1 part by mass of polyamide wax, 2 parts by mass of borax, 1 part by mass of potassium fluoride, and 89 parts by mass of Ag43CuZnNi solder powder (200 mesh~300 mesh).
[0094] [Comparative Example 2] This comparative example provides a shield cutter, and its preparation method is similar to that of Example 1, except that no coating material is applied to the cemented carbide surface of the shield cutter.
[0095] [Comparative Example 3] This comparative example provides a shield cutter, and its preparation method refers to Example 1, except that the working surface of the shield cutter is not coated with wear-resistant material.
[0096] [Comparative Example 4] This comparative example provides a shield cutter, and its preparation method is similar to that of Example 1, except that the hard alloy surface of the shield cutter is not coated with a coating material, and the working surface of the shield cutter is not coated with a wear-resistant material.
[0097] In order to compare and illustrate the difference in performance of the wear-resistant layer between the embodiment of the present invention and the comparative example, a shield cutter base body with a stress-bearing surface of 210 mm in length, 110 mm in width, and 220 mm in height, all of which were made of 42CrMo steel, was selected.
[0098] The shield blades of Examples 1-4 and Comparative Examples 1-4 were used as test objects for wear tests. The wear tests of the present invention were all conducted on the same wear test device. The wear test used clay layer slurry commonly used in shield blade engineering. The clay layer slurry was placed in the working tank. The shield blade was installed on the drive shaft, and the drive shaft was driven by a hydraulic motor to achieve rotary motion. The speed of the drive shaft was 10 r / min. The wear test time was 6 hours. The wear amount of the shield blade after the wear test was tested, and the results are shown in Table 1.
[0099] Table 1 Analysis results of examples and comparative examples Refer to Table 1 and Figure 8 , Comparative Example 1 uses a wear-resistant layer prepared with ordinary diamond. From Table 1, it can be seen that after the wear test of the shield cutter in Comparative Example 1, the wear amount of the shield cutter is measured to be 35.5 / g, indicating that the diamond is burned and carbonized; combined with Figure 8 It can be seen that the diamond in the wear-resistant layer is obviously carbonized. Fig. 9 In Example 1, the wear-resistant layer is prepared by using diamond activated by an activation liquid. From Table 1, it can be seen that after the wear test of the shield cutter in Example 1, the wear loss of the shield cutter is measured to be 23.5 / g, indicating that the coating layer is intact and the diamond is not burned; combined with Fig. 9 It can be seen that no carbide is found in the diamond in the prepared wear-resistant layer.
[0100] By comparing Example 1 and Comparative Example 1, it can be concluded that the activated diamond is not carbonized in an environment exceeding 700°C, so that the wear resistance of the diamond is increased, thereby increasing the wear resistance of the wear-resistant layer, and further improving the wear resistance of the shield cutter.
[0101] Continuing to compare Example 1 with Comparative Example 2, it can be seen from Table 1 that after the wear test of the shield blade in Example 1, the wear amount of the shield blade was measured to be 23.5 / g, and after the wear test of the shield blade in Comparative Example 2, the wear amount of the shield blade was measured to be 32.2 / g. However, no burning phenomenon was found in the hard alloy of the shield blade in Example 1, but after the wear test of the shield blade in Comparative Example 2, the hard alloy was found to be burned. By comparing Example 1 and Comparative Example 2, it can be concluded that after the trimethoxysilane is mixed with water, a hydrolysis reaction occurs to generate a coating material carrying a silanol group (-Si—OH), and then the coating material is applied to the surface of the hard alloy by the first paste dispenser 300; Fig.10 As shown in the figure, the coating material forms a dense nano-gel film on the surface of the cemented carbide. Through the energy spectrum analysis of the nano-gel film, the main component of the nano-gel film is SiO 2 , SiO 2The nanogel film can rely on its own cross-linking shrinkage stress to continuously and densely coat the surface of the cemented carbide, isolate the air on the surface of the cemented carbide to form a protective layer, thereby improving the high-temperature oxidation resistance of the cemented carbide.
[0102] Furthermore, the comparison principle between Examples 2-4 and Comparative Examples 2-3 is the same as the comparison principle between Example 1 and Comparative Example 1 above, and therefore, it will not be repeated here.
[0103] In this specification, the writing method of "S100", "S200" and "S300" is to facilitate the description of the embodiments of the present invention. The present invention can also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited by the order of the specific embodiments of the above writing method.
[0104] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A brazing method for a shield blade, the brazing method is used to prepare a shield blade, and the brazing method is applied to an automatic brazing production line, It is characterized in that The automatic brazing production line comprises a preheating furnace (100), a transition chamber (200), a welding chamber (500), and a first paste dispenser (300), and the brazing method comprises: S100: assembling an alloy steel matrix and a cemented carbide to obtain a tool matrix, and placing the tool matrix on a loading rack, which transports the tool matrix to the preheating furnace (100) for preheating treatment; S200: sending the tool substrate that has completed the preheating treatment into the transition chamber (200) to perform at least one gas washing operation; S300: pushing the tool base body after the gas washing operation into the welding chamber (500), and performing a first coating operation on the cemented carbide by the first paste dispenser (300); S400: performing a brazing operation on the tool substrate that has completed the first coating operation to obtain the shield tool.
2. The brazing method according to claim 1, It is characterized in that The automatic brazing production line further comprises a heat preservation furnace (600) and a second paste dispensing machine (400), and S400 specifically comprises: S410: the second paste dispensing machine (400) performs a second coating operation on the working surface of the tool base; S420: performing a wear-resistant brazing operation on the working surface that has completed the second coating operation; S430: sending the tool substrate that has completed the wear-resistant brazing operation into a heat preservation furnace (600) for gradient cooling.
3. The brazing method according to claim 2, It is characterized in that The S300 specifically includes: S310: mixing a first silane coupling agent and water to react once to obtain a coating material, and loading the coating material into the first paste dispensing machine (300); The S400 further includes: S440: preparing a wear-resistant material, and loading the wear-resistant material into the second paste dispensing machine (400).
4. The brazing method according to claim 3, It is characterized in that The temperature of the primary reaction is 20°C to 60°C; and / or The pressure of the primary reaction is 7MPa to 9MPa; and / or The time of the primary reaction is 30 to 50 minutes.
5. The brazing method according to claim 3, It is characterized in that The S440 specifically includes: S441: mixing the second silane coupling agent and water for a secondary reaction to obtain an intermediate product; S442: mixing the intermediate product, carboxyl boronic acid and catalyst A to react three times to obtain an activation solution; S443: mixing the activation solution with diamond, heating, and screening to obtain active diamond; S444: adding a solvent, a soldering flux, and a thixotropic agent into a reaction kettle, mixing and stirring, to obtain a soldering flux paste; S445: Mix and stir the active diamond, silver-based solder and the solder paste to obtain the wear-resistant material.
6. The brazing method according to claim 5, It is characterized in that The temperature of the secondary reaction is 40°C to 90°C; and / or The pressure of the secondary reaction is 7MPa to 9MPa; and / or The secondary reaction time is 25min to 35min; and / or The temperature of the three reactions is 60°C to 70°C; and / or The time of the three reactions is 1 h to 1.5 h; and / or The activation solution and the diamond are mixed and heated for 3 hours to 3.5 hours; and / or The activation solution is mixed with the diamond and heated at a temperature of 60° C. to 80° C.; and / or The temperature of adding the solvent, soldering flux and thixotropic agent into the reaction kettle for mixing and stirring is 90° C. to 150° C.; and / or The temperature for mixing and stirring the active diamond, the silver-based solder and the solder paste is 15° C. to 30° C.; and / or The time for mixing and stirring the active diamond, the silver-based solder and the soldering paste is 1.5 hours to 2.5 hours; and / or The vacuum degree of mixing and stirring the active diamond, silver-based solder and the solder paste is -80KPa to -100KPa.
7. A wear-resistant material for shield cutter, It is characterized in that The wear-resistant material is used in the brazing method according to any one of claims 1 to 6, and the wear-resistant material comprises: 2 to 8 parts by mass of active diamond powder; 4 to 10 parts by mass of active nanodiamond; 2 to 6 parts by mass of solvent; 1 to 3 parts by mass of thixotropic agent; 1 to 5 parts by mass of flux; 81 to 93 parts by mass of silver-based solder; Wherein, the silver-based solder is selected from at least one of Ag43CuZnNi, Ag40CuZnNiMn, Ag33CuZnSnNiMn, and Ag28CuZnNiMn.
8. The wear-resistant material according to claim 7, It is characterized in that The silver-based solder is a powder material, and the particle size of the powder material is 200 mesh to 300 mesh; and / or The particle size of the active diamond powder is 30 μm to 60 μm; and / or The particle size of the active nano-diamond is 100nm-200nm.
9. The wear-resistant material according to claim 7, It is characterized in that The solvent is selected from one or more of glycerol, fatty alcohol, and octanol; and / or The thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax; and / or The soldering flux is selected from one or more of borax and potassium fluoride.
10. An automatic brazing production line for shield cutters, It is characterized in that The automatic brazing production line adopts the brazing method according to any one of claims 1 to 6, and the automatic brazing production line comprises: A preheating furnace (100), the preheating furnace (100) being used to preheat the tool base body placed on a loading rack; A transition chamber (200), the transition chamber (200) being connected to the preheating furnace (100) and used for performing at least one gas washing operation on the tool base body that has completed the preheating treatment; A first paste dispensing machine (300), the first paste dispensing machine (300) being used to perform a first coating action on the cemented carbide of the tool substrate; A second paste dispensing machine (400), the second paste dispensing machine (400) being used to perform a second coating action on the working surface of the tool base; a welding chamber (500), the welding chamber (500) being arranged at one end of the transition chamber (200) away from the preheating furnace (100), and being used to perform a brazing action on the tool substrate that has completed the first coating action; A heat preservation furnace (600) is arranged at one end of the welding chamber (500) away from the transition chamber (200) and is used to perform gradient cooling on the shield cutter that has completed the brazing action.