Submerged arc welding process suitable for welding Ni series steel and 316L dissimilar steel

Through the submerged arc welding process, the problem of insufficient mechanical properties of the welded joints of Ni series steel and 316L dissimilar steel under low temperature conditions is solved, and good mechanical properties of the welded joints are achieved. It is suitable for Ni series steel and 316L dissimilar steel with a thickness of 16mm-40mm. Welded to meet low temperature impact and tensile strength requirements.

CN118768699APending Publication Date: 2024-10-15NANJING IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410846624.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult with the existing technology to make the joint between Ni series steel and 316L dissimilar steel meet the mechanical performance standards under low temperature conditions through welding process. In particular, the low temperature impact toughness is insufficient, which affects its application in structures such as storage and transportation of cryogenic storage tanks.

Method used

Submerged arc welding process is adopted. The specific steps include using symmetrical X-shaped arc welding groove, welding wire to connect Ni series steel and 316L dissimilar steel, welding current is 280A-350A, arc voltage is 21V-25V, and welding speed is 32cm/ min-38cm/min, the welding heat input is 10kJ/cm-16kJ/cm, and there is no preheating and root cleaning treatment to ensure the mechanical properties of the welded joint.

Benefits of technology

The low-temperature impact energy KV2 of the welded joint at -196°C is ≥34J, the tensile strength is ≥480MPa, and the longitudinal bending performance is qualified. It is suitable for the welding of 16mm-40mm thick Ni series steel and 316L dissimilar steel, forming good comprehensive mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768699A_ABST
    Figure CN118768699A_ABST
Patent Text Reader

Abstract

The invention discloses a submerged-arc welding process suitable for welding Ni-series steel and 316L dissimilar steel, which relates to the technical field of steel production, and comprises the following steps: connecting the Ni-series steel and the 316L dissimilar steel with a welding wire according to a submerged-arc welding form; a symmetrical X-shaped groove is adopted as an electric arc welding groove, the angle of the groove is 55-65 degrees, the length of a truncated edge is 1-3 mm, and the assembling gap of the groove is 1-3 mm; preheating is not conducted before welding, the interlayer temperature is smaller than or equal to 120 DEG C, and back gouging treatment is conducted before back face welding; submerged arc welding is adopted, the welding current ranges from 280 A to 350 A, the arc voltage ranges from 21 V to 25 V, the welding speed ranges from 32 cm / min to 38 cm / min, and the welding heat input ranges from 10 kJ / cm to 16 kJ / cm until welding is completed. A welded joint formed by the submerged-arc welding process provided by the invention has good comprehensive mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, and in particular to a submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel. Background Art

[0002] Ni-based steel is used for LNG tanks. In addition to the tank body itself, LNG tanks also need to be connected to feed pipes, accessories, etc. during construction. Generally, 316L stainless steel is used, which involves the connection of dissimilar materials. Ni-based steel and 316L dissimilar steel are connected by welding technology to form a structure used for storing and transporting cryogenic storage tanks. Whether the dissimilar steel welding has a wide welding process window, and whether the joint performance after welding, especially the low-temperature impact toughness of the welded joint, can meet the standards or user requirements, has become the first threshold for this type of steel to enter the market. Therefore, it is necessary to develop a submerged arc welding process suitable for the welding of Ni-based steel and 316L dissimilar steel, and to weld Ni-based steel and 316L dissimilar steel by submerged arc welding to ensure that the mechanical properties of the welded joint meet the requirements. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the disadvantages of the prior art and provide a submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel.

[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows: A submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel, comprising: Using submerged arc welding to connect Ni-based steel and 316L dissimilar steel; A symmetrical X-shaped groove is used as the arc welding groove, with a groove angle of 55°-65°, a blunt edge length of 1mm-3mm, and a groove assembly clearance of 1mm-3mm; No preheating before welding, the interlayer temperature is less than or equal to 120℃, and the back side is cleaned before welding; Submerged arc welding is used with a welding current of 280A-350A, an arc voltage of 21V-25V, a welding speed of 32cm / min-38cm / min, and a welding heat input of 10kJ / cm-16kJ / cm until the welding is completed.

[0005] As a preferred scheme of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the Ni-based steel includes the following components in weight percentage: C: 0.045%-0.060%, Mn: 0.50%-1.50%, Si: 0.10%-0.30%, S: ≤0.01%, P: ≤0.01%, Ni: 6.50%-8.00%, Mo: 0.20%-0.40%, and the balance is Fe and unavoidable impurities.

[0006] As a preferred scheme of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, wherein: the yield strength of the Ni-based steel is ≥580MPa, the tensile strength is ≥680MPa-820MPa, the elongation is ≥18%, and the impact energy KV2 at -196°C is ≥100J.

[0007] As a preferred solution of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the thickness of the Ni-based steel is 16mm-40mm.

[0008] As a preferred scheme of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the chemical composition and mass percentage of the 316L dissimilar steel are as follows: C: ≤0.04%, Mn: 0.50%-2.50%, Si: ≤0.90%, S: ≤0.02%, P: ≤0.03%, Ni: 11.0%-14.0%, Cr: 17.0%-20.0%, Mo: 0.3%-0.7%, Cu: ≤0.75%, and the balance is Fe and unavoidable impurities.

[0009] As a preferred solution of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, wherein: the yield strength of the 316L dissimilar steel is ≥177MPa, the tensile strength is ≥480MPa, the elongation is ≥40%, and the -196℃ impact energy KV2 is ≥34J.

[0010] As a preferred scheme of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the chemical composition and mass percentage of the welding wire are as follows: C: 0.20%-0.30%, Mn: 10.0%-12.0%, Si: 0.40%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~16%, W: 3.0%~4.0%, and the balance is Fe and unavoidable impurities.

[0011] As a preferred solution of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, the welding wire has a diameter of 2.4 mm, the low-temperature impact energy of the deposited metal at -196°C KV2≥48J, and the tensile strength≥600Mpa.

[0012] As a preferred solution of the submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel described in the present invention, wherein: after the submerged arc welding is completed, the low-temperature impact energy of the weld joint at -196°C KV2≥34J, the tensile strength of the weld joint≥480Mpa, the longitudinal surface bend d=4a, and 180° of the weld joint is qualified.

[0013] The beneficial effects of the present invention are: The submerged arc welding process provided by the present invention is easy to operate, and can ensure that the low-temperature impact energy KV2 of the welded joint (weld and heat-affected zone) at -196°C is ≥34J, the tensile strength of the welded joint is ≥480Mpa, and the longitudinal surface bending d=4a of the welded joint is qualified at 180°. The welded joint formed by the welding process has good comprehensive mechanical properties and is suitable for welding 16mm-40mm thick Ni-series steel and 316L dissimilar steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0015] Figure 1 Schematic diagram of welding Ni-based steel and 316L dissimilar steel provided by the present invention. DETAILED DESCRIPTION

[0016] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.

[0017] The present application provides a submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel, the process comprising the following steps: Step S101: Connect Ni-based steel and 316L dissimilar steel with welding wire in a submerged arc welding manner.

[0018] Specifically, the chemical composition and mass percentage of Ni-based steel are as follows: C: 0.045%-0.060%, Mn: 0.50%-1.50%, Si: 0.10%-0.30%, S: ≤0.01%, P: ≤0.01%, Ni: 6.50%-8.00%, Mo: 0.20%-0.40%, and the balance is Fe and unavoidable impurities.

[0019] Among them, the yield strength of Ni-based steel is ≥580MPa, the tensile strength is ≥680MPa-820MPa, the elongation is ≥18%, and the impact energy KV2 at -196℃ is ≥100J.

[0020] It should be noted that the present application is applicable to Ni-based steel with a thickness of 16 mm to 40 mm.

[0021] The chemical composition and mass percentage of 316L dissimilar steel are as follows: C: ≤0.04%, Mn: 0.50%-2.50%, Si: ≤0.90%, S: ≤0.02%, P: ≤0.03%, Ni: 11.0%-14.0%, Cr: 17.0%-20.0%, Mo: 0.3%-0.7%, Cu: ≤0.75%, the balance is Fe and unavoidable impurities.

[0022] Among them, the yield strength of 316L heterogeneous steel is ≥177MPa, the tensile strength is ≥480MPa, the elongation is ≥40%, and the impact energy KV2 at -196℃ is ≥34J.

[0023] The chemical composition and mass percentage of the welding wire are as follows: C: 0.20%-0.30%, Mn: 10.0%-12.0%, Si: 0.40%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~16%, W: 3.0%~4.0%, and the balance is Fe and unavoidable impurities.

[0024] Among them, the welding wire has a diameter of 2.4mm, the deposited metal has a low-temperature impact energy of -196℃ KV2≥48J, and a tensile strength of ≥600Mpa.

[0025] It should be noted that when selecting welding materials, the first consideration is to obtain a complete weld joint and ensure that the weld joint has a low-temperature impact energy of -196°C KV2 ≥ 34J and a tensile strength of ≥ 480MPa.

[0026] Step S102: using a symmetrical X-shaped groove as the arc welding groove, with a groove angle of 55°-65°, a blunt edge length of 1mm-3mm, and a groove assembly clearance of 1mm-3mm.

[0027] Step S103: No preheating before welding, the interlayer temperature is less than or equal to 120° C., and root cleaning is performed before reverse side welding.

[0028] Step S104: submerged arc welding is adopted, with a welding current of 280A-350A, an arc voltage of 21V-25V, a welding speed of 32cm / min-38cm / min, and a welding heat input of 10kJ / cm-16kJ / cm, until the welding is completed.

[0029] The submerged arc welding process applicable to the welding of Ni-based steel and 316L dissimilar steel is described below through a specific embodiment.

[0030] Embodiment 1: The arc welding process provided in this embodiment for welding Ni-based steel and 316L dissimilar steel comprises the following steps: The parent material is Ni-series steel with yield strength ≥580MPa, tensile strength ≥680MPa-820MPa, elongation ≥18%, and impact energy KV2 ≥100J at -196℃, and 316L with yield strength ≥177MPa, tensile strength ≥480MPa, elongation ≥40%, and impact energy KV2 ≥34J at -196℃, for butt welding. The welding test plate combination is 16mm+16mm, and the test plate size is 500mm (length) × 200mm (width) × 16mm (thickness).

[0031] The welding material is arc welding wire with a diameter of Φ2.4mm, the deposited metal has a low-temperature impact energy of -196℃ KV2≥48J, and a tensile strength≥600MPa. The welding wire includes the following components in weight percentage: C: 0.20%-0.30%, Mn: 10.0%-12.0%, Si: 0.40%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~16%, W: 3.0%~4.0%, and the balance is Fe and unavoidable impurities.

[0032] The groove form is an X-shaped groove, the groove angle is 55°, the blunt edge is 1mm, and the groove assembly clearance is 1mm.

[0033] No preheating before welding, the interlayer temperature is 65℃-100℃; the root is cleaned with a grinder before welding on the reverse side, and the root has a metallic luster.

[0034] Arc welding was used with a welding current of 280 A, an arc voltage of 21 V, a welding speed of 36 cm / min, and a welding heat input of 10 kJ / cm2 until the welding was completed. Embodiment 2: The arc welding process provided in this embodiment for welding Ni-based steel and 316L dissimilar steel comprises the following steps:

[0035] The parent material is Ni-series steel with yield strength ≥580MPa, tensile strength ≥680MPa-820MPa, elongation ≥18%, and impact energy KV2 ≥100J at -196℃, and 316L with yield strength ≥177MPa, tensile strength ≥480MPa, elongation ≥40%, and impact energy KV2 ≥34J at -196℃ for butt welding. The welding test plate combination is 30mm+30mm, and the test plate size is 500mm (length) × 200mm (width) × 30mm (thickness).

[0036] The welding material is arc welding wire with a diameter of Φ2.4mm, the deposited metal has a low-temperature impact energy of -196℃ KV2≥48J, and a tensile strength≥600MPa. The welding wire includes the following components in weight percentage: C: 0.20%-0.30%, Mn: 10.0%-12.0%, Si: 0.40%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~16%, W: 3.0%~4.0%, and the balance is Fe and unavoidable impurities.

[0037] The groove form is an X-shaped groove, the groove angle is 57°, the blunt edge is 2mm, and the groove assembly clearance is 1mm.

[0038] No preheating before welding, the interlayer temperature is 40℃-110℃; the root is cleaned with a grinder before welding on the reverse side, and the root has a metallic luster.

[0039] Arc welding was used with a welding current of 320 A, an arc voltage of 23 V, a welding speed of 34 cm / min, and a welding heat input of 13 kJ / cm2 until the welding was completed.

[0040] Embodiment 3: The arc welding process provided in this embodiment for welding Ni-based steel and 316L dissimilar steel comprises the following steps: The parent material is Ni-series steel with yield strength ≥580MPa, tensile strength ≥680MPa-820MPa, elongation ≥18%, and impact energy KV2 ≥100J at -196℃, and 316L with yield strength ≥177MPa, tensile strength ≥480MPa, elongation ≥40%, and impact energy KV2 ≥34J at -196℃. The welding test plate combination is 40mm+40mm, and the test plate size is 500mm (length) × 200mm (width) × 40mm (thickness).

[0041] The welding material is arc welding wire with a diameter of Φ2.4mm, the deposited metal has a low-temperature impact energy of -196℃ KV2≥48J, and a tensile strength≥600MPa. The welding wire includes the following components in weight percentage: C: 0.20%-0.30%, Mn: 10.0%-12.0%, Si: 0.40%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~16%, W: 3.0%~4.0%, and the balance is Fe and unavoidable impurities.

[0042] The groove form is an X-shaped groove, the groove angle is 58°, the blunt edge is 1mm, and the groove assembly clearance is 1mm.

[0043] No preheating before welding, the interlayer temperature is 42℃-100℃; the root is cleaned with a grinder before welding on the reverse side, and the root has a metallic luster.

[0044] Arc welding was used with a welding current of 350 A, an arc voltage of 25 V, a welding speed of 32 cm / min, and a welding heat input of 16 kJ / cm2 until the welding was completed.

[0045] The Ni-based steel and 316L dissimilar steel were welded by the welding method of the above-mentioned Examples 1-3, and the mechanical properties of the welded joints were tested. The impact, tensile and bending properties of the welded joints are shown in Tables 1 and 2:

[0046] Table 1: Impact performance of welded joints

[0047] Table 2: Tensile and lateral bending properties of welded joints It can be seen that the comprehensive mechanical properties of the welded joints obtained in Examples 1-3 are excellent. The impact energy of the weld and heat-affected zone at -196°C KV2≥34J, the tensile strength Rm:≥480MPa, and the longitudinal bend of the welded joint d=4a, 180° are qualified. In addition, the process implementation method provided by this patent is simple and has strong applicability.

[0048] Therefore, the technical solution provided by the present application is not only easy to operate, but also the welded joint formed by the welding process has good comprehensive mechanical properties.

[0049] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.

Claims

1. A submerged arc welding process suitable for welding Ni-based steel and 316L dissimilar steel, characterized in that: include: Using submerged arc welding to connect Ni-based steel and 316L dissimilar steel; A symmetrical X-shaped groove is used as the arc welding groove, with a groove angle of 55°-65°, a blunt edge length of 1mm-3mm, and a groove assembly clearance of 1mm-3mm; No preheating before welding, the interlayer temperature is less than or equal to 120℃, and the back side is cleaned before welding; Submerged arc welding is used with a welding current of 280A-350A, an arc voltage of 21V-25V, a welding speed of 32cm / min-38cm / min, and a welding heat input of 10kJ / cm-16kJ / cm until the welding is completed.

2. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1 is characterized in that: The Ni-based steel comprises the following components in weight percentage: C: 0.045%-0.060%, Mn: 0.50%-1.50%, Si: 0.10%-0.30%, S: ≤0.01%, P: ≤0.01%, Ni: 6.50%-8.00%, Mo: 0.20%-0.40%, and the balance is Fe and unavoidable impurities.

3. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 2 is characterized in that: The Ni-based steel has a yield strength of ≥580MPa, a tensile strength of ≥680MPa-820MPa, an elongation of ≥18%, and an impact energy KV2 of ≥100J at -196°C.

4. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, characterized in that: The thickness of the Ni-based steel is 16 mm to 40 mm.

5. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, characterized in that: The chemical composition and mass percentage of the 316L heterogeneous steel are as follows: C: ≤0.04%, Mn: 0.50%-2.50%, Si: ≤0.90%, S: ≤0.02%, P: ≤0.03%, Ni: 11.0%-14.0%, Cr: 17.0%-20.0%, Mo: 0.3%-0.7%, Cu: ≤0.75%, and the balance is Fe and unavoidable impurities.

6. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 5, characterized in that: The yield strength of the 316L heterogeneous steel is ≥177MPa, the tensile strength is ≥480MPa, the elongation is ≥40%, and the impact energy KV2 at -196°C is ≥34J.

7. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, characterized in that: The chemical composition and mass percentage of the welding wire are as follows: C: 0.20%-0.30%, Mn: 10.0%-12.0%, Si: 0.40%-0.60%, S: ≤0.01%, P: ≤0.02%, Ni: 12%~16%, W: 3.0%~4.0%, and the balance is Fe and unavoidable impurities.

8. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 6, characterized in that: The welding wire has a diameter of 2.4 mm, a low-temperature impact energy of the deposited metal of -196°C KV2≥48J, and a tensile strength≥600Mpa.

9. The submerged arc welding process for welding Ni-based steel and 316L dissimilar steel according to claim 1, characterized in that: After submerged arc welding is completed, the low-temperature impact energy of the weld joint at -196℃ KV2≥34J, the tensile strength of the weld joint≥480Mpa, the longitudinal bend of the weld joint d=4a, and 180° is qualified.

Citation Information

Patent Citations

  • Welding method for high manganese steel and 316L dissimilar steel

    CN116352235A

  • Submerged-arc welding process for marine-corrosion-resistant steel with yield strength of 420 MPa

    CN117206643A

  • Submerged arc welding process suitable for welding high manganese steel and 316L dissimilar steel

    CN117483926A

  • Submerged-arc welding process suitable for welding high-manganese steel and 9Ni dissimilar steel

    CN117548788A

  • Improvements in the production of wrought and cast steels and in articles produced therefrom and weld metals for use in the manufacture of weldments

    GB1076285A