Welding wire powder flux core, wear-resistant submerged arc surfacing flux-cored welding wire and preparation method and application of wear-resistant submerged arc surfacing flux-cored welding wire
By adding Nb element to the powder core of the welding wire and optimizing the steel strip structure, an NbC hard phase is formed, which solves the problem of easy peeling of the existing wear-resistant flux-cored welding wire and significantly improves the hardness and thermal stability of the cladding layer. Extends the service life of 60CrMnMo hot roll steel.
Patent Information
- Application Number
- CN202410939043.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The wear-resistant flux-cored wire used in existing surfacing repairs is prone to peeling off during the wear process, resulting in increased wear, and its high-temperature stability is not ideal.
A welding wire powder core including ferrochrome powder, ferroniobium powder, nickel powder, aluminum powder, activator, deoxidizer and rare earth oxide is used, and Nb element is added to form an NbC hard phase to improve toughness and hardness. And the wear resistance is enhanced through specific steel belt structure and welding process.
It effectively reduces the spalling of the welding layer, improves the hardness and thermal stability of the surfacing layer, extends the service life of the 60CrMnMo hot roll steel, avoids cracks on the roll surface during the welding process, and significantly improves the wear resistance.
Smart Images

Figure CN118768796A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding wires, and in particular to a welding wire powder core, a wear-resistant submerged arc cladding cored welding wire, and a preparation method and application thereof. Background Art
[0002] As steel production grows rapidly, the consumption of rolls is also increasing. In order to meet the rolling needs of steel products, the research and development of wear-resistant rolls has been accelerated.
[0003] 60CrMnMo is an alloy steel composed of carbon (C), chromium (Cr), manganese (Mn) and molybdenum (Mo). The addition of these elements makes 60CrMnMo have good strength and wear resistance. Due to its large volume and high replacement cost, 60CrMnMo roll steel can be repaired by surfacing welding to extend the service life of the roll body and reduce production costs.
[0004] At present, the wear-resistant flux-cored welding wire for surfacing repair generally contains alloy elements such as carbon, chromium, silicon, and manganese, and the chromium element occupies a higher proportion. 23 The high temperature stability of C6 is not ideal. It is extremely unstable and easy to aggregate at around 540℃, and it is very easy to peel off during the wear process, which aggravates the wear. Therefore, improving the wear resistance of flux-cored welding wire is an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a welding wire powder core, a wear-resistant submerged arc cladding flux-cored welding wire and a preparation method and application thereof, so as to solve the problem that the existing wear-resistant flux-cored welding wire repaired by cladding is very easy to peel off and aggravate wear.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A welding wire powder core comprises the following raw materials in percentage by weight:
[0008] Ferrochromium powder 25-46%, ferroniobium powder 10.5-26.5%, nickel powder 0.5-1.5%, aluminum powder 0.5-2%, activator 1-5%, deoxidizer 3-10%, rare earth oxide 0.1-1%, iron powder 12.5-38%.
[0009] Preferably, in the above-mentioned welding wire powder core, the activator is one or both of BaF and CaF2.
[0010] Preferably, in the above-mentioned welding wire powder core, the deoxidizer is one or both of ferrosilicon and ferromanganese.
[0011] Preferably, in the above-mentioned welding wire powder core, the rare earth oxide is one or both of La2O3 and Ce2O3.
[0012] The present invention also provides a wear-resistant submerged arc cladding flux-cored welding wire, comprising a steel strip and a welding wire powder flux core wrapped in the steel strip;
[0013] The welding wire powder core is the welding wire powder core mentioned above;
[0014] The filling rate of the welding wire powder core in the steel strip is 30-50%.
[0015] Preferably, in the above-mentioned wear-resistant submerged arc surfacing flux-cored welding wire, the steel strip is a H08A steel part.
[0016] The present invention also provides a method for preparing a wear-resistant submerged arc cladding flux-cored welding wire, comprising the following steps:
[0017] Mixing raw materials for preparing welding wire powder core to obtain a dry material mixture of welding wire powder core;
[0018] Rolling the steel strip into a U-shape to obtain a U-shaped steel strip;
[0019] The dry material mixture of the welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing the welding wire powder core is rolled into an O-shaped strip, and then drawn to obtain a wear-resistant submerged arc cladding flux-cored welding wire.
[0020] The invention also provides an application of a wear-resistant submerged arc surfacing flux-cored welding wire in hot-rolled roll steel materials.
[0021] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention adds Nb element to the powder core. Since Nb is a strong carbide-forming element and has a greater affinity for carbon than chromium, it can preferentially combine with carbon to form a NbC hard phase, generate a new wear-resistant phase, and can be evenly dispersed in the surfacing alloy, thereby refining the grains to reduce peeling, improving toughness, and improving the hardness of the surfacing layer, and enhancing the wear resistance and thermal stability of the surfacing layer. At the same time, the welding layer has good fusion with the base 60CrMnMo hot-rolled roller steel material and is firmly combined, which can prevent cracks from occurring on the roller surface during the welding process to affect the roller body quality, and extend the service life of the 60CrMnMo hot-rolled roller steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.
[0024] Figure 1The present invention is a flow chart for preparing the wear-resistant submerged arc cladding flux-cored welding wire;
[0025] Figure 2 The hardness distribution diagram of the wear-resistant submerged arc surfacing flux-cored welding wire surfacing layer and the base 60CrMnMo hot rolling roller steel material after surfacing the first layer, the second layer and the third layer in Application Example 1;
[0026] Figure 3 The friction coefficient diagram of the wear-resistant submerged arc cladding flux-cored wire cladding layer in Application Example 1;
[0027] Figure 4 The appearance and wear weight loss diagram of the wear-resistant submerged arc cladding flux-cored wire cladding layer and the base 60CrMnMo hot rolling roller steel material before and after wear in Application Example 1;
[0028] Figure 5 The microstructure diagram of the interface between the base 60CrMnMo hot-rolled roller steel material and the wear-resistant submerged arc cladding flux-cored welding wire cladding layer in Application Example 1;
[0029] Figure 6 This is the microstructure diagram of the wear-resistant submerged arc cladding flux-cored wire cladding layer in Application Example 1. DETAILED DESCRIPTION
[0030] A welding wire powder core comprises the following raw materials in percentage by weight:
[0031] Ferrochromium powder 25-46%, ferroniobium powder 10.5-26.5%, nickel powder 0.5-1.5%, aluminum powder 0.5-2%, activator 1-5%, deoxidizer 3-10%, rare earth oxide 0.1-1%, iron powder 12.5-38%.
[0032] In the present invention, the mass percentage of the ferrochrome powder is preferably 25-46%, more preferably 28-40%, and even more preferably 35-38%.
[0033] In the present invention, the mass percentage of the ferroniobium powder is preferably 10.5-26.5%, more preferably 15-24%, and even more preferably 18-21%.
[0034] In the present invention, the mass percentage of the nickel powder is preferably 0.5-1.5%, more preferably 0.6-1.2%, and more preferably 0.8-1%.
[0035] In the present invention, the mass percentage of the aluminum powder is preferably 0.5-2%, more preferably 0.6-1.5%, and even more preferably 1-1.2%.
[0036] In the present invention, the mass percentage of the active agent is preferably 1-5%, more preferably 2-4%, and even more preferably 2.5-3%.
[0037] In the present invention, the mass percentage of the deoxidizer is preferably 3-10%, more preferably 4-8%, and even more preferably 5-6%.
[0038] In the present invention, the mass percentage of the rare earth oxide is preferably 0.1-1%, more preferably 0.2-0.8%, and even more preferably 0.5-0.6%.
[0039] In the present invention, the mass percentage of the iron powder is preferably 12.5 to 38%, more preferably 15 to 36%, and even more preferably 20 to 30%.
[0040] In the present invention, the composition of the ferrochrome powder is: Cr 60.0% to 80.0wt%, C≤10wt%, Si≤3wt%, and the balance is Fe. The ferrochrome powder serves as a transition alloy element to the cladding alloy.
[0041] In the present invention, the composition of the ferroniobium powder is: Nb 50.0% to 70.0wt%, C≤0.1wt%, Si≤3wt%, Al≤3wt%, and the balance is Fe. The ferroniobium powder preferentially combines with carbon in the cladding layer to form a NbC hard wear-resistant phase.
[0042] In the present invention, the nickel powder and aluminum powder are used to improve the hardenability of the cladding alloy.
[0043] In the present invention, the activator is preferably one or both of BaF and CaF2, more preferably BaF. The activator is used to eliminate pores in the molten pool and improve the welding performance of the cladding alloy.
[0044] In the present invention, the deoxidizer is preferably one or both of ferrosilicon and ferromanganese, more preferably ferrosilicon;
[0045] The ferrosilicon comprises 60.0% to 80.0% by weight of Si, 0.01% to 0.1% by weight of C, and the balance is Fe;
[0046] The composition of the ferromanganese is Mn 70-90wt%, Si 1-5wt%, C 0.1-1wt%, and the balance is Fe. The function of the deoxidizer is to increase the strength and hardness of the cladding metal by deoxidizing silicon and manganese, and silicon and manganese are both strong deoxidizers. The deoxidation effect is more ideal by using silicon and manganese combined deoxidation.
[0047] In the present invention, the rare earth oxide is preferably one or both of La2O3 and Ce2O3, and more preferably La2O3. The role of the rare earth oxide is to refine the cladding alloy structure and make the carbides more evenly distributed in the matrix.
[0048] In the present invention, the iron powder serves to supplement alloy elements to the surfacing alloy.
[0049] The present invention also provides a wear-resistant submerged arc cladding flux-cored welding wire, comprising a steel strip and a welding wire powder flux core wrapped in the steel strip;
[0050] The welding wire powder core is the welding wire powder core mentioned above;
[0051] The filling rate of the welding wire powder core in the steel strip is 30-50%, more preferably 32-45%, and even more preferably 33-40%.
[0052] In the present invention, the steel strip is preferably a H08A steel piece.
[0053] In the present invention, the diameter of the wear-resistant submerged arc cladding flux-cored welding wire is preferably 2.4 to 4 mm, more preferably 2.5 to 3.8 mm, and more preferably 3 to 3.5 mm.
[0054] The present invention also provides a method for preparing a wear-resistant submerged arc cladding flux-cored welding wire, comprising the following steps:
[0055] Mixing raw materials for preparing welding wire powder core to obtain a dry material mixture of welding wire powder core;
[0056] Rolling the steel strip into a U-shape to obtain a U-shaped steel strip;
[0057] The dry material mixture of the welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing the welding wire powder core is rolled into an O-shaped strip, and then drawn to obtain a wear-resistant submerged arc cladding flux-cored welding wire.
[0058] In the present invention, the pretreatment of the raw materials for preparing the welding wire powder core is drying, and the drying temperature is preferably 180-250°C, more preferably 190-240°C, and more preferably 200-210°C; the drying time is 1.5-3h, more preferably 1.75-2.5h, and more preferably 2h.
[0059] In the present invention, the specific method of mixing is: stirring and mixing in a V-type powder mixer; the mixing time is preferably ≥120 min, more preferably 120 to 200 min, and more preferably 150 min.
[0060] The preparation process flow chart of wear-resistant submerged arc cladding flux-cored wire is as follows Figure 1 shown.
[0061] The invention also provides an application of a wear-resistant submerged arc surfacing flux-cored welding wire in hot-rolled roll steel materials.
[0062] In the present invention, the hot rolling roll steel material is preferably 60CrMnMo hot rolling roll steel material.
[0063] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] Example 1
[0065] A wear-resistant submerged arc cladding flux-cored welding wire, comprising an outer steel strip and a powder flux core wrapped by the steel strip; the filling rate of the powder flux core in the steel strip is 33%; the steel strip is made of H08A steel;
[0066] The welding wire powder core includes the following raw materials in percentage by weight:
[0067] Ferrochrome powder 28%, ferroniobium powder 21%, nickel powder 1%, aluminum powder 1%, activator 2%, deoxidizer 10%, rare earth oxide 1%, iron powder 36%;
[0068] The composition of the ferrochrome powder is: Cr 70wt%, C 8.5wt%, Si 0.6wt%, and the balance is Fe;
[0069] The composition of the ferroniobium powder is: Nb 65wt%, C 0.07wt%, Si 2.6wt%, Al 1.5wt%, and the balance is Fe;
[0070] The active agent is BaF;
[0071] The deoxidizer is a mixture of ferrosilicon and ferromanganese, with the mass ratio of ferrosilicon to ferromanganese being 1:10;
[0072] The composition of the ferrosilicon is Si 74wt%, C 0.05wt%, and the balance is Fe;
[0073] The composition of the ferromanganese is 80wt% Mn, 1.35wt% Si, 0.1wt% C, and the balance is Fe;
[0074] The rare earth oxide is a mixture of La2O3 and Ce2O3; the mass ratio of La2O3 to Ce2O3 is 1:1;
[0075] The method for preparing the wear-resistant submerged arc cladding flux-cored welding wire comprises the following steps:
[0076] The raw materials for preparing the welding wire powder core are dried at 200° C. for 2 hours, and then the dried raw materials are added into a V-type powder mixer and stirred for 150 minutes to obtain a dry material mixture of the welding wire powder core;
[0077] The steel strip H08A steel product is rolled into a U-shape to obtain a U-shaped steel strip;
[0078] The dry material mixture of the welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing the powder core is rolled into an O-shape, and then drawn to obtain a wear-resistant submerged arc cladding flux-cored welding wire with a diameter of 3 mm.
[0079] Application Example 1
[0080] The surface of the 60CrMnMo hot-rolled roller steel material was polished with coarse sandpaper, and then the surface was cleaned with anhydrous ethanol to obtain the treated 60CrMnMo hot-rolled roller steel material; the automatic submerged arc welding machine used the wear-resistant submerged arc surfacing flux-cored welding wire prepared in Example 1 as the welding material to perform the first layer of surfacing on the surface of the treated 60CrMnMo hot-rolled roller steel material, and after surfacing the first layer, the heat was kept for one minute before the second layer of surfacing was started; after surfacing the second layer, the heat was kept for one minute before the third layer of surfacing was performed, and after the surfacing of the third layer was completed, the 60CrMnMo hot-rolled roller steel material and the surfacing alloy formed by surfacing were cooled to room temperature in the air to complete the welding, and a wear-resistant submerged arc surfacing flux-cored welding wire surfacing layer was formed on the 60CrMnMo hot-rolled roller steel material; wherein the conditions for the first layer of surfacing, the second layer of surfacing and the third layer of surfacing were: welding current of 380A, voltage of 30V, welding speed of 360mm / min, and wire feeding speed of 500mm / min.
[0081] Figure 2 This is the hardness distribution diagram of the wear-resistant submerged arc surfacing flux-cored wire surfacing layer and the base 60CrMnMo hot rolling roller steel material after surfacing the first layer, the second layer, and the third layer in Application Example 1. Figure 2 It can be seen that the base 60CrMnMo hot-rolled roller steel material has the lowest hardness. As the number of surfacing layers increases, the hardness of the wear-resistant submerged arc surfacing flux-cored wire surfacing layer gradually increases, and the maximum hardness is reached when the surfacing reaches the third layer. Figure 2 The horizontal axis in the figure represents the points for measuring hardness from the substrate to the cladding layer in sequence. The first 4 points are hit on the substrate, 5-13 are hit on the first cladding layer, 14-21 are hit on the second cladding layer, and 22-30 are hit on the third cladding layer.
[0082] Figure 3 This is the friction coefficient diagram of the wear-resistant submerged arc cladding flux-cored wire cladding layer in Application Example 1. Figure 3 It can be seen that at the beginning of wear, the friction coefficient rises sharply, and stabilizes after 1 minute, with the friction coefficient being 0.35. In the subsequent wear process, the friction coefficient remains basically unchanged.
[0083] Figure 4 This is the appearance and wear weight loss diagram of the wear-resistant submerged arc cladding flux-cored wire cladding layer and the base 60CrMnMo hot rolling roller steel material before and after wear in Application Example 1. Figure 4 It can be seen that after the wear test, the wear weight loss of the cladding alloy is very small, only 0.0001 grams, while the wear weight loss of the substrate is higher.
[0084] Figure 5 This is the microstructure diagram of the interface between the base 60CrMnMo hot-rolled roller steel material and the wear-resistant submerged arc cladding flux-cored wire cladding layer in Application Example 1. Figure 5 It can be seen that the left side is the 60CrMnMo hot-rolled steel plate substrate, and the right side is the surfacing layer. The interface bonding is good and there is no cracking.
[0085] Figure 6 This is the microstructure of the wear-resistant submerged arc cladding flux-cored wire cladding layer in Application Example 1. Figure 6 It can be seen that a large amount of black precipitates are precipitated in the microstructure, which are detected to be NbC.
[0086] According to the above results, it can be known that the wear-resistant submerged arc cladding flux-cored welding wire of the present invention has good welding process performance, the surface hardness of the cladding layer is evenly distributed, the average hardness is 650HV, and the wear resistance is 15 times that of the substrate.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A welding wire powder core, characterized in that: Including the following raw materials in percentage by weight: Ferrochromium powder 25-46%, ferroniobium powder 10.5-26.5%, nickel powder 0.5-1.5%, aluminum powder 0.5-2%, activator 1-5%, deoxidizer 3-10%, rare earth oxide 0.1-1%, iron powder 12.5-38%.
2. The welding wire powder core according to claim 1, characterized in that: The active agent is one or both of BaF and CaF2.
3. The welding wire powder core according to claim 2, characterized in that: The deoxidizer is one or both of ferrosilicon and ferromanganese.
4. The welding wire powder core according to claim 3, characterized in that: The rare earth oxide is one or both of La2O3 and Ce2O3.
5. A wear-resistant submerged arc cladding flux-cored welding wire, characterized in that: It comprises a steel strip and a welding wire powder core wrapped in the steel strip; The welding wire powder core is the welding wire powder core according to any one of claims 1 to 4; The filling rate of the welding wire powder core in the steel strip is 30-50%.
6. The wear-resistant submerged arc cladding flux-cored welding wire according to claim 5, characterized in that: The steel belt is made of H08A steel.
7. The method for preparing the wear-resistant submerged arc cladding flux-cored welding wire according to claim 5 or 6, characterized in that: The following steps are involved: Mixing raw materials for preparing welding wire powder core to obtain a dry material mixture of welding wire powder core; Rolling the steel strip into a U-shape to obtain a U-shaped steel strip; The dry material mixture of the welding wire powder core is filled into a U-shaped steel strip, and then the U-shaped steel strip containing the welding wire powder core is rolled into an O-shaped strip, and then drawn to obtain a wear-resistant submerged arc cladding flux-cored welding wire.
8. Use of the wear-resistant submerged arc cladding flux-cored welding wire according to claim 5 or 6 in hot-rolled roll steel materials.
Citation Information
Patent Citations
Niobium enhanced wear-resisting submerged arc bead weld flux-cored wire
CN101856776A
Self-shielded flux-cored welding wire for super-high niobium content strengthening and toughening surfacing and preparation method thereof
CN106166654A
AU2021102205A4
Cited By
Flux-cored wire with high crack resistance and wear resistance and preparation method of flux-cored wire
CN119747957A