Welding wire for E-grade cast steel welding and E-grade cast steel welding method

Through welding wires and welding processes with specific components, the problems of hot cracking tendency and low efficiency in welding of E-grade cast steel are solved, and high mechanical properties and high-efficiency welding effects are achieved. The tensile strength and impact absorption energy at room temperature are significantly improved. Seam hardness and hardness are also improved.

CN118768797APending Publication Date: 2024-10-15CRRC INDUSTRAIL ACADEMY (QINGDAO) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410899256.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

Smart Images

  • Figure BDA0004930028130000051
    Figure BDA0004930028130000051
  • Figure BDA0004930028130000061
    Figure BDA0004930028130000061
  • Figure BDA0004930028130000071
    Figure BDA0004930028130000071
Patent Text Reader

Abstract

The invention provides a welding wire for E-grade cast steel welding and a welding method of the E-grade cast steel. The welding wire comprises the following components of 0.05%-0.1% of C, 1.8%-2.1% of Mn, 0.6%-1.0% of Si, 2.2%-2.8% of Ni, 0.6%-0.9% of Mo, 0.4%-0.8% of Cr, 0.05%-0.1% of Ti, 0.2%-0.6% of Cu, 1.5%-2.4% of Ce, smaller than or equal to 0.02% of S, smaller than or equal to 0.02% of P and the balance Fe. The welding wire with the components is used for welding E-grade cast steel, on one hand, the hot crack tendency of a welding seam can be remarkably improved, and the welding seam can still be controlled to be free of obvious crack defects under the conditions that the low preheating temperature and the high interlayer temperature are kept and the postweld heat treatment step is not included; and on the other hand, the effects of deoxidation, desulfurization and generation of a strengthening phase through reaction can be achieved, so that weld joints are purified, grains are refined, the performance is strengthened, and the mechanical performance of a welded joint is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and in particular relates to a welding wire for welding E-grade cast steel and an E-grade cast steel welding method. Background Art

[0002] In recent years, with the continuous increase in high-speed rail speed and passenger capacity, higher requirements have been placed on train manufacturing materials. In order to meet the requirements of heavy load and speed increase of my country's trains, the materials of many key components have been gradually upgraded from traditional C-grade cast steel to E-grade cast steel with better mechanical properties, and some components are even made entirely of E-grade cast steel.

[0003] However, compared with the weldability of C-grade cast steel, E-grade cast steel has a tendency to harden, a serious tendency to welding thermal cracks and a large welding internal stress. Traditional E-grade steel welding can only rely on the use of high-strength welding rods such as J857 and J707, which requires a high preheating temperature, strict control of the lower interlayer temperature, interlayer grinding and complex post-weld tempering heat treatment procedures, and the welding efficiency is slow and the mechanical properties of the welded joints are poor. Therefore, it is urgent to solve the problems of welding cracking, complex process, low efficiency and poor joint performance of E-grade cast steel. Summary of the invention

[0004] In view of this, an object of the present invention is to provide a welding wire for E-grade cast steel welding and an E-grade cast steel welding method, wherein the E-grade cast steel weld welded by the welding wire has no crack defects and good mechanical properties.

[0005] The present invention provides a welding wire for E-grade cast steel welding, which comprises the following components by mass fraction:

[0006] C0.05~0.1%, Mn1.8~2.1%, Si0.6~1.0%, Ni2.2~2.8%, Mo0.6~0.9%, Cr0.4~0.8%, Ti0.05~0.1%, Cu0.2~0.6%, Ce1.5~2.4%, S≤0.02%, P≤0.02%, balance Fe.

[0007] The present invention provides a method for welding E-grade cast steel, comprising the following steps:

[0008] Use grinding technology to clean the groove;

[0009] Preheat the workpiece, the preheating temperature is not higher than 200℃, and the holding time is 15 to 30 minutes;

[0010] The workpiece is welded by using the welding wire described in the above technical solution; the weld structure is multi-layer and multi-pass, and the inter-layer temperature of the welding is 350-410°C;

[0011] After natural cooling, E grade cast steel is obtained after welding.

[0012] Preferably, the heat input used in welding is 0.7-1.2 KJ / mm.

[0013] Preferably, the preheating temperature is 150-190°C.

[0014] Preferably, the welding conditions include:

[0015] The welding atmosphere is 84% ​​Ar and 16% CO 2 Mixed gas, gas flow rate is 12-15L / min;

[0016] The welding current is 230~260A, the arc voltage is 27.3~27.6V; the power supply polarity is DC EP / +.

[0017] Preferably, the weld structure adopts 4 layers and 12 passes;

[0018] The first layer is Lane 1;

[0019] The second layer includes lanes 2, 3, and 4;

[0020] The third level includes lanes 5, 6, 7, and 8;

[0021] The fourth layer includes lanes 9, 10, 11 and 12.

[0022] Preferably, the tensile strength of the E-grade cast steel after welding at room temperature is 860-920 MPa, the impact absorption energy at -40°C is 65-70 J; the hardness at the weld is 260-270 HV 10 , heat affected zone hardness 260~265HV 10 .

[0023] The present invention provides a welding wire for welding E-grade cast steel, which comprises the following components by mass fraction: C 0.05-0.1%, Mn 1.8-2.1%, Si 0.6-1.0%, Ni 2.2-2.8%, Mo 0.6-0.9%, Cr 0.4-0.8%, Ti 0.05-0.1%, Cu 0.2-0.6%, Ce 1.5-2.4%, S ≤ 0.02%, P ≤ 0.02%, and the balance Fe. The present invention adopts the welding wire comprising the Ce element and other components to weld E-grade cast steel, which can significantly improve the thermal cracking tendency of the weld on the one hand, and can still control the weld to have no obvious crack defects under the condition of maintaining the low preheating temperature, the high-layer temperature and not including the post-weld heat treatment step; on the other hand, it can also play the role of deoxidation, desulfurization and reaction to generate strengthening phase, so as to purify the weld, refine the grains and strengthen the performance, and improve the mechanical properties of the weld joint. The experimental results show that the tensile strength of the welded joint at room temperature is 860-920 MPa, and the fracture is located in the parent material; the impact absorption energy is 65-70 J (-40 ° C); the hardness of the weld is 260-270 HV 10 , heat affected zone hardness 260~265HV 10 . BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The welding sequence used for welding in the present invention;

[0025] Figure 2 is a metallographic diagram of the welded joint in Example 1 of the present invention;

[0026] Figure 3 This is a metallographic diagram of the welded joint in Example 2 of the present invention. DETAILED DESCRIPTION

[0027] The present invention provides a welding wire for E-grade cast steel welding, which comprises the following components by mass fraction:

[0028] C0.05~0.1%, Mn1.8~2.1%, Si0.6~1.0%, Ni2.2~2.8%, Mo0.6~0.9%, Cr0.4~0.8%, Ti0.05~0.1%, Cu0.2~0.6%, Ce1.5~2.4%, S≤0.02%, P≤0.02%, balance Fe.

[0029] The present invention adopts the above-mentioned welding wire including Ce element and other components to weld E-grade cast steel. On the one hand, it can significantly improve the thermal cracking tendency of the weld. Under the above-mentioned conditions of maintaining low preheating temperature, high-layer temperature and not including post-weld heat treatment steps, the weld can still be controlled to have no obvious crack defects; on the other hand, it can also play the role of deoxidation, desulfurization and reaction to generate strengthening phases, thereby purifying the weld, refining the grains and strengthening the performance, and improving the mechanical properties of the weld joint.

[0030] The present invention provides a method for welding E-grade cast steel, comprising the following steps:

[0031] Use grinding technology to clean the groove;

[0032] Preheat the workpiece, the preheating temperature is not higher than 200℃, and the holding time is 15 to 30 minutes;

[0033] The workpiece is welded by using the welding wire described in the above technical solution; the weld structure is multi-layer and multi-pass, and the inter-layer temperature of the welding is 350-410°C;

[0034] After natural cooling, E grade cast steel is obtained after welding.

[0035] The welding process provided by the present invention is simple, has low equipment requirements, low manufacturing cost, etc. The process includes groove cleaning, workpiece preheating, welding, etc.

[0036] The present invention adopts a grinding process to clean the groove and remove oil stains and rust.

[0037] The present invention preheats the pretreated workpiece. The present invention preferably places the workpiece in a resistance furnace for preheating; the preheating temperature is not higher than 200°C, preferably 150-190°C; the insulation time is 15-30 minutes. The lower the preheating temperature, the more conducive to improving welding efficiency and saving energy. However, the more serious the tendency of weld cracks, the conventional preheating temperature before welding is higher than 200°C to inhibit welding cracks. The present invention uses a welding wire composed of specific components, a lower preheating temperature, and a welding process combined with specific process conditions, which will not cause welding cracks.

[0038] The present invention adopts the welding wire described in the above technical solution to weld the workpiece; the weld structure is multi-layer and multi-pass, and the inter-layer temperature of welding is 350-410°C.

[0039] In the present invention, the temperature between welding layers is controlled to be 350-410°C; the higher the temperature between welding layers, the more important it is for improving welding efficiency, but too high an interlayer temperature will lead to a large heat input to the weld, coarsening of weld grains, and reduced weld strength; the present invention adopts the welding wire of the above composition and controls the temperature between welding layers, so that the weld has a higher tensile strength.

[0040] The present invention strictly controls the welding heat input; the heat input used in welding is 0.7-1.2 KJ / mm.

[0041] The welding conditions described in the present invention include:

[0042] The welding atmosphere is 84% ​​Ar and 16% CO 2 Mixed gas, gas flow rate is 12-15L / min;

[0043] The welding current is 230~260A, the arc voltage is 27.3~27.6V; the power supply polarity is DC EP / +.

[0044] The weld structure of the present invention adopts 4 layers and 12 passes; the welding sequence is as follows: Figure 1 As shown:

[0045] The first layer is Lane 1;

[0046] The second layer includes lanes 2, 3, and 4;

[0047] The third level includes lanes 5, 6, 7, and 8;

[0048] The fourth layer includes lanes 9, 10, 11 and 12.

[0049] The present invention does not require heat treatment after welding, and natural cooling is sufficient, and an E-grade cast steel joint with good weld quality can still be obtained.

[0050] The present invention adopts GB / T 228 standard method to test the tensile strength of the joint, adopts GB / T 229 standard method to test the impact absorption work of the joint, and adopts GB / T 4340.2 standard method to test the hardness of the weld joint and the heat affected zone.

[0051] Through the implementation of the present invention, the welding efficiency of E-grade cast steel is greatly improved by more than 1 times compared with the welding efficiency of traditional high-strength steel electric welding rods such as J857 and J707, and energy is saved. The weld has no crack defects and has good mechanical properties: the tensile strength at room temperature is 860-920MPa, and the fracture is located in the parent material; the impact absorption energy is 65-70J (-40℃); the hardness at the weld is 260-270HV 10 , heat affected zone hardness 260~265HV 10 .

[0052] In order to further illustrate the present invention, a welding wire for welding E-grade cast steel and an E-grade cast steel welding method provided by the present invention are described in detail below in combination with embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0053] Example 1

[0054] Before welding, the groove is cleaned by grinding to remove oil and rust;

[0055] Place the workpiece in a resistance furnace for preheating at 150°C and a holding time of 15 minutes;

[0056] The welding material is the high-strength steel gas shielded welding wire shown in Table 1. The welding wire composition is shown in Table 1. The shielding gas composition is 84% ​​Ar + 16% CO 2 , gas flow rate is 12L / min, power polarity is DC EP / +, welding current is controlled between 230-260A for different passes, arc voltage is controlled between 27.3-27.6V, welding heat input is strictly controlled between 0.7-1.2KJ / mm, weld structure adopts 4 layers and 12 passes; welding sequence is as follows Figure 1 The welding process parameters are shown in Table 2:

[0057] After welding one layer, proper cooling is required. It is only necessary to control the temperature between welding layers within the range of 350-410℃.

[0058] Allow to cool naturally after welding.

[0059] Table 1 Composition of high strength steel gas shielded welding wire (%)

[0060] C Mn Si S P Ni Mo Cr Ti Cu Ce Fe 0.05 1.8 0.65 ≤0.02 ≤0.02 2.25 0.6 0.4 0.05 0.2 1.5 margin

[0061] Table 2 Process parameters of different welding passes

[0062]

[0063] Figure 2 This is a metallographic diagram of the welded joint prepared in Example 1 of the present invention; it can be seen that the welded joint has a good metallurgical bonding effect, and has no defects such as cracks and pores. The tensile strength of the E-grade cast steel at room temperature after welding is 882Mpa, and the impact absorption energy at -40°C is 67J; the hardness at the weld is 265HV 10 , the hardness of the heat affected zone is 262HV 10 .

[0064] Example 2

[0065] Before welding, the groove is cleaned by grinding to remove oil and rust;

[0066] Place the workpiece in a resistance furnace for preheating at 190°C for 30 minutes;

[0067] The welding material is the high-strength steel gas shielded welding wire shown in Table 3, and the welding wire composition is shown in Table 1; the shielding gas composition is 84% ​​Ar + 16% CO 2, gas flow rate is 14L / min, power polarity is DC EP / +, welding current is controlled between 235-258A for different passes, arc voltage is controlled between 27.3-27.5V, welding heat input is strictly controlled between 0.7-1.2KJ / mm, weld structure adopts 4 layers and 12 passes; welding sequence is as follows Figure 1 The welding process parameters are shown in Table 4:

[0068] After welding one layer, proper cooling is required. It is only necessary to control the temperature between welding layers within the range of 350-410℃.

[0069] Allow to cool naturally after welding.

[0070] Table 3 Composition of high strength steel gas shielded welding wire (%)

[0071] C Mn Si S P Ni Mo Cr Ti Cu Ce Fe 0.95 2.1 1.0 ≤0.02 ≤0.02 2.75 0.85 0.8 0.1 0.6 2.4 margin

[0072] Table 4 Process parameters of different welding passes

[0073]

[0074] Figure 3 This is a metallographic diagram of the welded joint prepared in Example 2 of the present invention; it can be seen that the welded joint has a good metallurgical bonding effect, and has no defects such as cracks and pores. The tensile strength of the E-grade cast steel at room temperature after welding is 918Mpa, and the impact absorption energy at -40°C is 67J; the hardness at the weld is 268HV 10 , the hardness of the heat affected zone is 263HV 10 .

[0075] Example 3

[0076] Before welding, the groove is cleaned by grinding to remove oil and rust;

[0077] Place the workpiece in a resistance furnace for preheating at 170°C and a holding time of 25 minutes;

[0078] The welding material is the high-strength steel gas shielded welding wire shown in Table 5, and the welding wire composition is shown in Table 1; the shielding gas composition is 84% ​​Ar + 16% CO 2 , gas flow rate is 14L / min, power polarity is DC EP / +, welding current is controlled between 230-260A for different passes, arc voltage is controlled between 27.3-27.5V, welding heat input is strictly controlled between 0.7-1.2KJ / mm, weld structure adopts 4 layers and 12 passes; welding sequence is as follows Figure 1 The welding process parameters are shown in Table 6:

[0079] After welding one layer, proper cooling is required. It is only necessary to control the temperature between welding layers within the range of 350-410℃.

[0080] Allow to cool naturally after welding.

[0081] Table 5 Composition of high strength steel gas shielded welding wire (%)

[0082] C Mn Si S P Ni Mo Cr Ti Cu Ce Fe 0.65 1.9 0.95 ≤0.02 ≤0.02 2.55 0.8 0.55 0.1 0.55 2.2 margin

[0083] Table 6 Process parameters of different welding passes

[0084]

[0085] After metallographic inspection, the welded joint has good metallurgical bonding effect, without cracks, pores and other defects. The tensile strength of E-grade cast steel at room temperature after welding is 905Mpa, the impact absorption energy at -40℃ is 69J; the hardness at the weld is 266HV 10 , the hardness of the heat affected zone is 261HV 10 .

[0086] It can be seen from the above embodiments that the present invention provides a welding wire for welding E-grade cast steel, which includes the following components by mass fraction: C0.05-0.1%, Mn1.8-2.1%, Si0.6-1.0%, Ni2.2-2.8%, Mo0.6-0.9%, Cr0.4-0.8%, Ti0.05-0.1%, Cu0.2-0.6%, Ce1.5-2.4%, S≤0.02%, P≤0.02%, and the balance Fe. The present invention uses the welding wire including the Ce element and other components to weld E-grade cast steel. On the one hand, it can significantly improve the thermal cracking tendency of the weld. Under the above-mentioned conditions of maintaining low preheating temperature, high inter-layer temperature and not including the post-weld heat treatment step, it can still control the weld to have no obvious crack defects; on the other hand, it can also play the role of deoxidation, desulfurization and reaction to generate strengthening phases, thereby purifying the weld, refining the grains and strengthening the performance, and improving the mechanical properties of the weld joint. The experimental results show that the tensile strength of the welded joint at room temperature is 860-920 MPa, and the fracture is located in the parent material; the impact absorption energy is 65-70 J (-40 ° C); the hardness of the weld is 260-270 HV 10 , heat affected zone hardness 260~265HV 10 .

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A welding wire for welding grade E cast steel, comprising the following components by mass fraction: C0.05~0.1%, Mn1.8~2.1%, Si0.6~1.0%, Ni2.2~2.8%, Mo0.6~0.9%, Cr0.4~0.8%, Ti0.05~0.1%, Cu0.2~0.6%, Ce1.5~2.4%, S≤0.02%, P≤0.02%, balance Fe.

2. A method for welding E-grade cast steel, comprising the following steps: Use grinding technology to clean the groove; Preheat the workpiece, the preheating temperature is not higher than 200℃, and the holding time is 15 to 30 minutes; The welding wire according to claim 1 is used to weld the workpiece; the weld structure is multi-layer and multi-pass, and the inter-layer temperature of the welding is 350-410°C; After natural cooling, E grade cast steel is obtained after welding.

3. The method according to claim 2, characterized in that The heat input used in welding is 0.7~1.2KJ / mm.

4. The method according to claim 2, characterized in that: The preheating temperature is 150-190°C.

5. The method according to claim 2, characterized in that: The welding conditions include: The welding atmosphere is a mixture of 84% Ar and 16% CO2, with a gas flow rate of 12-15 L / min; The welding current is 230~260A, the arc voltage is 27.3~27.6V; the power supply polarity is DC EP / +.

6. The method according to claim 2, characterized in that The weld structure adopts 4 layers and 12 passes; The first layer is Lane 1; The second layer includes lanes 2, 3, and 4; The third level includes lanes 5, 6, 7, and 8; The fourth layer includes lanes 9, 10, 11 and 12.

7. The method according to claim 2, characterized in that The tensile strength of E-grade cast steel after welding is 860-920 MPa at room temperature, the impact absorption energy is 65-70 J at -40 ° C, and the hardness at the weld is 260-270 HV 10 , heat affected zone hardness 260~265HV 10 .