Ceramic sand roll special for steel rail polishing and preparation method of ceramic sand roll

By preparing special ceramic sand rolls for rail grinding with high wear resistance and high temperature resistance, the problems of short service life and high cost of existing sand rolls are solved, and efficient and safe rail grinding effects are achieved.

CN118769085AActive Publication Date: 2024-10-15SHAOGUAN WEIMING ABRASIVE MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411092334.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-15
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Existing rail grinding abrasive rolls have a short service life and high costs, and rely on imported high-quality abrasive rolls, resulting in efficiency and price issues.

Method used

A method of preparing special ceramic sand rolls for rail grinding is adopted, including base cloth pretreatment, PVA phenolic resin mixture impregnation, back scraping layer and multi-layer coating treatment to form a ceramic with high wear resistance, high temperature resistance and high sharpness. Sand roll.

Benefits of technology

A ceramic sand roll with high wear resistance, high temperature resistance and high sharpness is realized, which extends the service life and reduces the processing cost. It is suitable for grinding high-speed rail rails, prevents burns and deformation, and improves grinding efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769085A_ABST
    Figure CN118769085A_ABST
Patent Text Reader

Abstract

The invention provides a ceramic sand roll special for steel rail grinding and a preparation method thereof, and belongs to the technical field of sand roll machining. The preparation method of the ceramic sand roll special for steel rail polishing comprises the steps that firstly, pretreated base cloth is soaked in PVA phenolic resin mixed liquid and dried, back scraping treatment is conducted to form a back scraping layer, then the front face is sequentially coated with a pre-coating layer, a primer layer, a gravity sand planting layer, an electrostatic adsorption abrasive particle layer, a composite glue layer and an ultra-coating layer, and finally the ceramic sand roll special for steel rail polishing is obtained through curing and flexing. And the ceramic sand roll special for steel rail polishing is obtained. The abrasive roll is suitable for manufacturing a single-joint abrasive belt, is good in heat absorption and burn prevention performance during grinding, is suitable for long-term grinding operation of a high-speed rail without sand falling, deformation and extension, is beneficial to eliminating the burn phenomenon of the rail, and is beneficial to stable use of the abrasive belt. The abrasive belt prepared by adopting the abrasive roll can achieve the purpose of protecting the surface of the steel rail, and has the characteristics of high cutting force, long service life, high sharpness and efficient and rapid polishing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of abrasive roll processing, and in particular to a ceramic abrasive roll specially used for rail grinding and a preparation method thereof. Background Art

[0002] Rail grinding is a maintenance work that is essential to ensure the safety of railway transportation. After a long period of train travel, the rail surface may have defects or unevenness, which will reduce the running stability and safety of the rail, and also increase the wear of the rail and wheels. Therefore, rail grinding is necessary to improve safety, reduce maintenance costs, and extend service life.

[0003] The reasons for rail grinding usually include the following:

[0004] Removing surface defects: With the increase of service time, cracks, peeling, indentations and other defects will appear on the surface of the rail, which need to be removed by grinding.

[0005] Smooth surface: Long-term use will cause wavy lines and unevenness on the rail surface. Grinding can restore the surface flatness and improve driving stability.

[0006] Improve track geometry: Grinding can correct track geometry, such as track gauge, track shape, and track surface verticality, to meet track specification requirements.

[0007] Improve drainage capacity: A good track surface can enhance the drainage capacity of the track, prevent water accumulation on the railway line, and reduce problems such as slippery and muddy coverage.

[0008] At present, the service life of conventional abrasive belts is generally low. Frequent replacement of abrasive belts during work not only reduces efficiency, but also increases costs. High-quality ceramic abrasive belts for rails mainly rely on imported abrasive rolls, such as 3M, VSM, etc. These brands of abrasive rolls have good quality and high efficiency, but are expensive, 3 to 5 times the price of other brands of abrasive rolls. Therefore, how to develop a high-quality abrasive roll for rail grinding and reduce its processing cost is a major research direction at present. Summary of the invention

[0009] In view of this, the purpose of the present invention is to provide a method for preparing ceramic abrasive rolls for rail grinding, wherein the abrasive rolls prepared by the method have the characteristics of high wear resistance, high hardness, high temperature resistance, high sharpness, fine surface treatment and maintaining the geometry of the track.

[0010] In order to achieve the above object, the present invention provides a method for preparing a ceramic abrasive roll specially used for rail grinding, the preparation method comprising the following steps:

[0011] (1) Pretreatment of the base fabric: the base fabric is subjected to inspection, repair, curling, singeing and high-temperature shaping treatment; the high-temperature shaping treatment is to subject the base fabric to high-temperature shaping in a high-temperature shaping machine at a temperature of 160-220°C; the base fabric is a pure polyester grey fabric.

[0012] (2) mixing a PVA aqueous solution and a phenolic resin to obtain a PVA phenolic resin mixed solution; then dipping the base fabric pretreated in step (1) in the mixed solution, drying the base fabric after the dipping treatment at 120-180° C. for 1-3 minutes and then setting it aside;

[0013] (3) using a back-scratching layer to perform back-scratching treatment on the back side of the dried base fabric, and drying at 80-180° C. for 1-4 minutes to form a back-scratching layer;

[0014] (4) Apply a pre-coating layer to the front of the base fabric and dry it; then apply a primer layer, a gravity sanding layer and an electrostatic adsorption abrasive layer and dry it; then apply a re-sizing layer and a super coating layer and dry it again;

[0015] (5) After drying, a curing treatment is performed, and finally, the ceramic sand roll for rail grinding is obtained by kneading and rolling;

[0016] The pre-coating layer in step (4) is composed of the following raw materials in parts by weight: 45-75 parts of phenolic resin, 20-40 parts of heavy calcium carbonate, and 0.1-1 parts of leveling agent; the particle size of the heavy calcium carbonate is 400 mesh or 800 mesh.

[0017] Preferably, the mass concentration of the PVA aqueous solution in step (2) is 15-25wt%; and the mass ratio of the PVA aqueous solution to the phenolic resin is 1:1 to 1:5.

[0018] Preferably, the back-scratching layer in step (3) is composed of the following raw materials in parts by weight: 25-45 parts of phenolic resin, 15-30 parts of acrylic resin, 20-50 parts of 800 mesh heavy calcium carbonate, 1-5 parts of color paste, and 0.5-1 part of emulsifier.

[0019] Preferably, the drying temperature in step (4) is 85-120° C. and the drying time is 60-120 min.

[0020] Preferably, the base glue layer in step (4) is composed of the following raw materials in parts by weight: 40-75 parts of phenolic resin, 30-50 parts of heavy calcium carbonate, and 0.1-1 part of silane coupling agent; the particle size of the heavy calcium carbonate is 400 mesh or 800 mesh.

[0021] Preferably, the gravity-planted sand in step (4) is calcined brown corundum with a particle size of 70-800 μm;

[0022] The electrostatic abrasive layer is composed of thick sheet or strip nanocrystalline ceramic corundum abrasives, and the particle size of the nanocrystalline ceramic corundum abrasives is 100-1000 microns.

[0023] Preferably, the compound glue in step (4) is composed of the following raw materials in parts by weight: 40-65 parts of phenolic resin, 30-80 parts of cryolite, 1-3 parts of color paste, and 0-0.5 parts of silane coupling agent; the particle size of the cryolite is 400 mesh or 800 mesh.

[0024] Preferably, the super coating in step (4) is composed of the following raw materials in parts by weight: 5-20 parts of epoxy resin, 10-30 parts of polyimide, 1-5 parts of color paste, 0-70 parts of 400 mesh cryolite, 25-60 parts of potassium fluoroborate, 0.5-1.5 parts of silane coupling agent, and 5-10 parts of ethylene glycol ether.

[0025] Preferably, the curing temperature in step (5) is 120° C. and the curing time is 5-40 hours.

[0026] In the preparation process of the present invention, the thickness of the base fabric plus the back-scratching layer is 0.7-0.8 mm, and the coating amount of the remaining layers is:

[0027] Pre-coating 60~200g / m 2 , Base glue layer 100~500g / m 2 , Gravity sand planting layer 80~500g / m 2 , Electrostatic sand planting layer 150~1000g / m 2 , adhesive layer 100~650g / m 2 , Super coating 80~700g / m 2 .

[0028] Another object of the present invention is to provide a special ceramic sand roll for rail grinding prepared by the above method, which comprises, from top to bottom, a super coating layer, a double glue layer, an electrostatic sand planting layer, a gravity sand planting layer, a base glue layer, a pre-coating layer, a base cloth layer, and a back scraping layer.

[0029] The functions of each layer are as follows: the super coating prevents burns; the double adhesive layer fixes the sand and cloth; the base adhesive layer provides glue to make the sand stick to the cloth surface; the pre-coating layer increases the flatness of the cloth surface, prevents sand from peeling off, and increases the service life of the sand roll.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention provides a special ceramic sand roll for rail grinding and a preparation method thereof. The sand roll of the present invention is suitable for making a single-joint sanding belt, and has good heat absorption and anti-burning performance during grinding. It is suitable for long-term operation of high-speed rail grinding without sand loss, deformation, or extension, which is beneficial to eliminating rail burns and is beneficial to the stable use of the sanding belt. The sanding belt prepared by the sand roll of the present invention can achieve the purpose of protecting the surface of the rail, and has the characteristics of high cutting force, long service life, high sharpness, and efficient and fast grinding. The sanding belt prepared by the special ceramic sand roll for rail grinding of the present invention has the following properties:

[0032] With high wear resistance, high hardness and high temperature resistance, ceramic abrasive belts can withstand heavy loads, are not easy to wear, and have low temperatures during grinding, making them suitable for grinding heavy-load infrastructure.

[0033] High sharpness: Ceramic abrasive belts can quickly grind rails and improve work efficiency.

[0034] Fine surface treatment: Ceramic abrasive belts can produce very fine surfaces, meeting the fineness required for railway safety and operation.

[0035] Maintain track geometry: Ceramic abrasive belts can accurately remove uneven parts, maintain the track geometry, and ensure smooth and safe railway operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic diagram of the structure of a ceramic sand roll specifically used for rail grinding according to an embodiment of the present invention;

[0037] Figure 2 This is a schematic diagram of the structure of a special ceramic sand roll for rail grinding in this comparative method;

[0038] Figure 3 This is a microscopic photograph of the strip-shaped nanocrystalline ceramic corundum in Example 1;

[0039] Figure 4 This is a micrograph of the ordinary ceramic corundum in Comparative Example 5.

[0040] Serial number description: 1-1 super coating layer; 1-2 double adhesive layer; 1-3 electrostatic sanding layer; 1-4 gravity sanding layer; 1-5 base adhesive layer; 1-6 pre-coating layer; 1-7 base fabric layer; 1-8 back scraping layer;

[0041] 2-1 super coating layer; 2-2 double adhesive layer; 2-3 electrostatic sand planting layer; 2-4 gravity sand planting layer; 2-5 base adhesive layer; 2-6 base fabric layer; 2-7 back scraping layer. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with the embodiments.

[0043] In a specific embodiment of the present invention, the phenolic resins used are all produced by Taier Phenolic Resin (Guangdong) Co., Ltd., and are phenolic resins of model P805155A low-aldehyde (P16B), P805158A (P11) or P805150A low-aldehyde (P1A), whose main component is water-soluble liquid phenolic resin; the silane coupling agent is KH-792 silane coupling agent produced by Shuguang Company, and the emulsifier is sorbitan monococoate; the dispersant is the emulsifier Span S-20 purchased from Hai'an Petrochemical Plant in Jiangsu Province; the black color paste is P050 black color paste purchased from Shiming Technology; the blue color paste is A21 blue color paste purchased from Shiming Technology. The strip-shaped nanocrystalline ceramic corundum abrasive with a diameter of 800 microns described in the embodiment is the Receramax PRO ceramic abrasive purchased from Qingdao Reker New Material Technology Co., Ltd.; the ordinary ceramic corundum abrasive with a diameter of 800 microns described in the comparative example is the Receramax RE ceramic abrasive purchased from Qingdao Reker New Material Technology Co., Ltd.; the zirconium corundum is zirconium corundum AZ40 purchased from Saint-Gobain Ceramic Materials (Zhengzhou) Co., Ltd.

[0044] In a specific embodiment of the present invention, the thickness of the base fabric plus the back-scratching layer is 0.7-0.8 mm, and the coating amount of the remaining layers is:

[0045] Pre-coating 100g / m 2 , Base glue layer 200g / m 2 , Gravity sand planting layer 300g / m 2 , Electrostatic sand planting layer 600g / m 2 , adhesive layer 200g / m 2 , Super coating 100g / m 2 .

[0046] In the embodiments of the present invention, raw materials are generally purchased products unless otherwise specified, and preparation methods are generally prepared by conventional methods in the art unless otherwise specified.

[0047] Example 1

[0048] A special ceramic sand roll for rail grinding, the preparation method is as follows:

[0049] (1) Fabric pretreatment: The fabric is inspected, repaired, rolled, singed and subjected to high-temperature setting treatment; the high-temperature setting treatment is to set the fabric in a high-temperature setting machine at a temperature of 195°C;

[0050] (2) A 20 wt % PVA aqueous solution and a phenolic resin P805155A low-formaldehyde (P16B) are mixed in a mass ratio of 1:4 to obtain a PVA phenolic resin mixed solution, and then the base fabric pretreated in step (1) is immersed in the mixed solution, and the base fabric immersed in the PVA phenolic resin mixed solution is dried at 150° C. for 2 minutes for standby use;

[0051] (3) using a back-scratching layer to perform back-scratching treatment on the back side of the dried base fabric, and drying at 150° C. for 3 minutes to form a back-scratching layer;

[0052] (4) applying a pre-coating layer to the front side of the base fabric and drying; then applying a primer layer, a gravity sanding layer and an electrostatic adsorption abrasive layer and drying; then applying a secondary glue layer and a super coating layer and drying again, the drying temperature is 115° C. and the drying time is 60 min;

[0053] (5) After drying, the ceramic sand roll for rail grinding is obtained by curing in a curing furnace at a temperature of 120°C for 20 hours and finally by kneading and rolling.

[0054] The base fabric is all polyester grey fabric;

[0055] The back-scratching layer is composed of the following raw materials in parts by weight: 35 parts of phenolic resin P805155A low-aldehyde (P16B), 25 parts of acrylic resin, 36.3 parts of 800-mesh heavy calcium carbonate, 3 parts of black color paste, and 0.7 parts of emulsifier.

[0056] The pre-coat layer is composed of the following raw materials in parts by weight: 65 parts of phenolic resin P805150A low aldehyde (P1A), 34.5 parts of 800 mesh heavy calcium carbonate, and 0.5 parts of leveling agent.

[0057] The primer is prepared by mixing the following raw materials in parts by weight: 55 parts of phenolic resin P805158A (P11), 44.5 parts of 800-mesh heavy calcium carbonate, and 0.5 parts of a silane coupling agent.

[0058] The gravity sand layer is calcined corundum with a particle size of 650 microns.

[0059] The compound glue is composed of the following raw materials in parts by weight: 45 parts of phenolic resin P805158A (P11), 52.5 parts of 800-mesh cryolite, 2 parts of blue color paste, and 0.5 parts of silane coupling agent.

[0060] The super coating is composed of the following raw materials in parts by weight: 10 parts of epoxy resin, 10 parts of polyimide, 2 parts of blue color paste, 40 parts of 400-mesh cryolite, 32 parts of potassium fluoroborate, 1 part of silane coupling agent, and 5 parts of ethylene glycol ether;

[0061] The electrostatic abrasive layer is composed of strip-shaped nanocrystalline ceramic corundum abrasive with a particle diameter of 800 microns.

[0062] Ceramic sand rolls for rail grinding, from top to bottom, are super coating, double glue layer, electrostatic abrasive layer, gravity sand planting layer, base glue layer, pre-coating layer, base cloth layer, back scraping layer, such as Figure 1 , in which the electrostatic sand-planting layer is evenly distributed in the super coating layer, the double glue layer and the base glue layer, and protrudes from the surface of the sand roll.

[0063] Example 2

[0064] A special ceramic sand roll for rail grinding, the preparation method is as follows:

[0065] (1) Fabric pretreatment: The fabric is inspected, repaired, rolled, singed and subjected to high-temperature setting treatment; the high-temperature setting treatment is to set the fabric in a high-temperature setting machine at a temperature of 190°C;

[0066] (2) A 22 wt % PVA aqueous solution and a phenolic resin P805155A low-formaldehyde (P16B) are mixed in a mass ratio of 1:4.5 to obtain a PVA phenolic resin mixed solution, and then the base fabric pretreated in step (1) is immersed in the mixed solution, and the base fabric immersed in the PVA phenolic resin mixed solution is dried at 155° C. for 2 minutes for standby use;

[0067] (3) using a back-scratching layer to perform back-scratching treatment on the back side of the dried base fabric, and drying at 150° C. for 3 minutes to form a back-scratching layer;

[0068] (4) applying a pre-coating layer to the front side of the base fabric and drying; then applying a primer layer, a gravity sanding layer and an electrostatic adsorption abrasive layer and drying; then applying a secondary glue layer and a super coating layer and drying again, the drying temperature is 110° C. and the drying time is 70 min;

[0069] (5) After drying, the ceramic sand roll for rail grinding is obtained by curing in a curing furnace at a temperature of 120°C for 20 hours and finally by kneading and rolling.

[0070] The base fabric is all polyester grey fabric;

[0071] The back-scratching layer is composed of the following raw materials in parts by weight: 40 parts of phenolic resin P805155A low-aldehyde (P16B), 20 parts of acrylic resin, 36.5 parts of 800-mesh heavy calcium carbonate, 3 parts of black color paste, and 0.5 parts of emulsifier.

[0072] The pre-coat layer is composed of the following raw materials in parts by weight: 60 parts of phenolic resin P805150A low aldehyde (P1A), 39.5 parts of 800 mesh heavy calcium carbonate, and 0.5 parts of leveling agent.

[0073] The primer is prepared by mixing the following raw materials in parts by weight: 50 parts of phenolic resin P805158A (P11), 49.5 parts of 800-mesh heavy calcium carbonate, and 0.5 parts of a silane coupling agent.

[0074] The gravity sand layer is calcined corundum with a particle size of 650 microns.

[0075] The compound glue is composed of the following raw materials in parts by weight: 40 parts of phenolic resin P805158A (P11), 57.5 parts of 800-mesh cryolite, 2 parts of blue color paste, and 0.5 parts of silane coupling agent.

[0076] The super coating is composed of the following raw materials in parts by weight: 15 parts of epoxy resin, 10 parts of polyimide, 2 parts of blue color paste, 30 parts of 400-mesh cryolite, 37 parts of potassium fluoroborate, 1 part of silane coupling agent, and 5 parts of ethylene glycol ether;

[0077] The electrostatic abrasive layer is composed of strip-shaped nanocrystalline ceramic corundum abrasive with a particle diameter of 800 microns.

[0078] Ceramic sand rolls for rail grinding, from top to bottom, are super coating, double glue layer, electrostatic abrasive layer, gravity sand planting layer, base glue layer, pre-coating layer, base cloth layer, back scraping layer, such as Figure 1 .

[0079] Example 3

[0080] A special ceramic sand roll for rail grinding, the preparation method is as follows:

[0081] (1) Fabric pretreatment: The fabric is inspected, repaired, rolled, singed and subjected to high-temperature setting treatment; the high-temperature setting treatment is to set the fabric in a high-temperature setting machine at a temperature of 190°C;

[0082] (2) A 25 wt % PVA aqueous solution and a phenolic resin P805155A low-formaldehyde (P16B) are mixed in a mass ratio of 1:5 to obtain a PVA phenolic resin mixed solution, and then the base fabric pretreated in step (1) is immersed in the mixed solution, and the base fabric immersed in the PVA phenolic resin mixed solution is dried at 140° C. for 3 minutes for standby use;

[0083] (3) using a back-scratching layer to perform back-scratching treatment on the back side of the dried base fabric, and drying at 150° C. for 3 minutes to form a back-scratching layer;

[0084] (4) applying a pre-coating layer to the front side of the base fabric and drying; then applying a primer layer, a gravity sanding layer and an electrostatic adsorption abrasive layer and drying; then applying a secondary glue layer and a super coating layer and drying again, the drying temperature is 115° C. and the drying time is 70 min;

[0085] (5) After drying, the ceramic sand roll for rail grinding is obtained by curing in a curing furnace at a temperature of 120°C for 20 hours and finally by kneading and rolling.

[0086] The base fabric is all polyester grey fabric;

[0087] The back-scratching layer is composed of the following raw materials in parts by weight: 40 parts of phenolic resin P805155A low-aldehyde (P16B), 15 parts of acrylic resin, 41.5 parts of 800-mesh heavy calcium carbonate, 3 parts of black color paste, and 0.5 parts of emulsifier.

[0088] The pre-coat layer is composed of the following raw materials in parts by weight: 55 parts of phenolic resin P805150A low aldehyde (P1A), 44.5 parts of 800 mesh heavy calcium carbonate, and 0.5 parts of leveling agent.

[0089] The primer is prepared by mixing the following raw materials in parts by weight: 55 parts of phenolic resin P805158A (P11), 44 parts of 800-mesh heavy calcium carbonate, and 1 part of silane coupling agent.

[0090] The gravity sand layer is calcined corundum with a particle size of 650 microns.

[0091] The compound glue is composed of the following raw materials in parts by weight: 42 parts of phenolic resin P805158A (P11), 56 parts of 800-mesh cryolite, 1.5 parts of blue color paste, and 0.5 parts of silane coupling agent.

[0092] The super coating is composed of the following raw materials in parts by weight: 10 parts of epoxy resin, 15 parts of polyimide, 2 parts of blue color paste, 35 parts of 400-mesh cryolite, 32 parts of potassium fluoroborate, 1 part of silane coupling agent, and 5 parts of ethylene glycol ether;

[0093] The electrostatic abrasive layer is composed of strip-shaped nanocrystalline ceramic corundum abrasive with a particle diameter of 800 microns.

[0094] Ceramic sand rolls for rail grinding, from top to bottom, are super coating, double glue layer, electrostatic abrasive layer, gravity sand planting layer, base glue layer, pre-coating layer, base cloth layer, back scraping layer, such as Figure 1 .

[0095] Comparative Example 1

[0096] A ceramic abrasive roll specially used for rail grinding is prepared by the same method as in Example 1, except that the abrasive roll in Comparative Example 1 does not include a pre-coating layer.

[0097] The structure of the special ceramic sand roll for rail grinding is as follows Figure 2 From top to bottom, they are super coating, double adhesive layer, electrostatic sand planting layer, gravity sand planting layer, base adhesive layer, base cloth layer and back scraping layer. The electrostatic sand planting layer is evenly distributed in the super coating, double adhesive layer and base adhesive layer, and protrudes from the surface of the sand roll.

[0098] Comparative Example 2

[0099] A zirconium corundum abrasive roll specially used for metal polishing is prepared by the same method as in Example 1, except that Comparative Example 2 does not include a super coating, and the electrostatic abrasive layer of Comparative Example 2 is composed of zirconium corundum abrasive with a particle diameter of 800 microns.

[0100] Comparative Example 3

[0101] A ceramic abrasive roll specially used for rail grinding is prepared by the same method as in Example 1, except that the pre-coating raw material in Comparative Example 3 does not contain a leveling agent.

[0102] Comparative Example 4

[0103] A ceramic abrasive roll specially used for rail grinding is prepared by the same method as in Example 1, except that the super coating raw material in Comparative Example 4 does not contain a silane coupling agent.

[0104] Comparative Example 5

[0105] A ceramic abrasive roll specially used for rail grinding is prepared in the same manner as in Example 1, except that the electrostatic abrasive layer in Comparative Example 5 is composed of common ceramic corundum abrasive with a particle diameter of 800 microns.

[0106] The sand rolls prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were cut and made into single-joint sand belts for performance testing, including wear resistance (meters of rails ground per hour, reflecting the service life of the sand belt), hardness (microhardness Vickers), high temperature resistance (grinding the rail surface for 1 hour, blue represents burns), breaking strength (N / cm), and 600N longitudinal elongation (the lower the less likely it is to deform). The results are shown in Table 1:

[0107] Table 1

[0108]

[0109]

[0110] It can be seen from Table 1 that the abrasive belt prepared without adding a pre-coating layer in Comparative Example 1 has poor wear resistance. This result is because the abrasive grains of the abrasive belt without a pre-coating layer are easy to fall off, which reduces the friction properties and service life of the abrasive belt.

[0111] In Comparative Example 2, zirconium corundum abrasive was used without super coating, resulting in insufficient abrasive sharpness, decreased grinding force, and a very short service life without the high temperature protection of the super coating. The wear resistance was less than 50% of that of Example 1.

[0112] In the pre-coating of Comparative Example 3, no leveling agent was used, and the overall breaking strength decreased by 10%, and the service life was also reduced by 10-15%.

[0113] In the super coating of comparative example 4, no silane coupling agent is used, the elongation increases by 40%, the deformation is relatively large, the service life decreases by 20%, and because the super coating formula is changed, the high temperature resistance is reduced.

[0114] The abrasive used in Comparative Example 5 is common ceramic corundum, which has poor sharpness and reduces wear resistance.

[0115] Microscopic analysis was performed on the strip-shaped nanocrystalline ceramic corundum in Example 1 and the common ceramic corundum in Comparative Example 5, and microscopic photographs of the strip-shaped nanocrystalline ceramic corundum were obtained as shown in FIG. Figure 3 ; Microscopic photos of common ceramic corundum such as Figure 4 It can be seen that the strip-shaped nanocrystalline ceramic corundum used in Example 1 has a higher sharpness.

[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a special ceramic abrasive roll for rail grinding, characterized in that: The preparation method comprises the following steps: (1) Fabric pretreatment: inspect, repair, curl, singe and perform high-temperature shaping on the fabric; (2) mixing a PVA aqueous solution and a phenolic resin to obtain a PVA phenolic resin mixed solution; then dipping the base fabric pretreated in step (1) in the mixed solution, drying the base fabric after the dipping treatment at 120-180° C. for 1-3 minutes and then setting it aside; (3) using a back-scratching layer to perform back-scratching treatment on the back side of the dried base fabric, and drying at 80-180° C. for 1-4 minutes to form the back-scratching layer; (4) Apply a pre-coating layer to the front of the base fabric and dry it; then apply a primer layer, a gravity sand planting layer and an electrostatic adsorption abrasive layer and dry it; then apply a re-sizing layer and a super coating layer and dry it again; (5) After drying, a curing treatment is performed, and finally, the ceramic sand roll for rail grinding is obtained by kneading and rolling; The pre-coating layer in step (4) is composed of the following raw materials in parts by weight: 45-75 parts of phenolic resin, 20-40 parts of heavy calcium carbonate, and 0.1-1 parts of leveling agent; the particle size of the heavy calcium carbonate is 400 mesh or 800 mesh.

2. The method for preparing the special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The mass concentration of the PVA aqueous solution in step (2) is 15-25wt%; the mass ratio of the PVA aqueous solution to the phenolic resin is 1:1 to 1:

5.

3. The method for preparing the special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The back-scratching layer in step (3) is composed of the following raw materials in parts by weight: 25-45 parts of phenolic resin, 15-30 parts of acrylic resin, 20-50 parts of 800 mesh heavy calcium carbonate, 1-5 parts of color paste, and 0.5-1 part of emulsifier.

4. The method for preparing the special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The drying temperature in step (4) is 85-120° C. and the drying time is 60-120 min.

5. The method for preparing the special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The base glue layer in step (4) is composed of the following raw materials in parts by weight: 40-75 parts of phenolic resin, 30-50 parts of heavy calcium carbonate, and 0.1-1 parts of silane coupling agent; the particle size of the heavy calcium carbonate is 400 mesh or 800 mesh.

6. The method for preparing the special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The gravity planting sand in step (4) is calcined brown corundum with a particle size of 70-800 microns; The electrostatic abrasive layer is composed of thick sheet or strip nanocrystalline ceramic corundum abrasives, and the particle size of the nanocrystalline ceramic corundum abrasives is 100-1000 microns.

7. The method for preparing a special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The compound glue in step (4) is composed of the following raw materials in parts by weight: 40-65 parts of phenolic resin, 30-80 parts of cryolite, 1-3 parts of color paste, and 0-0.5 parts of silane coupling agent; the particle size of the cryolite is 400 mesh or 800 mesh.

8. The method for preparing the special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The super coating in step (4) is composed of the following raw materials in parts by weight: 5-20 parts of epoxy resin, 10-30 parts of polyimide, 1-5 parts of color paste, 0-70 parts of 400 mesh cryolite, 25-60 parts of potassium fluoroborate, 0.5-1.5 parts of silane coupling agent, and 5-10 parts of ethylene glycol ether.

9. The method for preparing a special ceramic abrasive roll for rail grinding according to claim 1, characterized in that: The curing temperature in step (5) is 120° C. and the curing time is 5-40 hours.

10. A special ceramic abrasive roll for rail grinding, characterized in that: The ceramic sand roll is prepared by any one of the methods of claims 1 to 9, wherein the ceramic sand roll comprises, from top to bottom, a super coating layer, a double adhesive layer, an electrostatic sand planting layer, a gravity sand planting layer, a base adhesive layer, a pre-coating layer, a base cloth layer, and a back-scraping layer.

Citation Information

Patent Citations

  • Abrasive cloth special for soft cloth hardware water mill automatic machine and preparation method of abrasive cloth

    CN117798838A

  • Abrasive cloth special for descaling stainless steel plate and preparation method of abrasive cloth

    CN117798839A

  • Liquid infused surface-modified material

    WO2024083812A1