High-performance shell-imitated structure wood and preparation method thereof

Cell swelling and esterification of poplar wood through lithium hydroxide and dimethyl sulfoxide solutions, combined with vacuum impregnation and inorganic salt mineralization processes of ammonium dihydrogen phosphate and magnesium chloride, form imitation shell structure wood, solving the problem of fast-growing wood strength deficiencies and chemical treatment safety issues, enabling the preparation of high-performance wood.

CN118769342AActive Publication Date: 2024-10-15NORTHEAST FORESTRY UNIV

Patent Information

Application Number
CN202411084591.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-15
Estimated Expiration
2044-08-08

Smart Images

  • Figure CN118769342A_ABST
    Figure CN118769342A_ABST
Patent Text Reader

Abstract

The invention discloses high-performance shell-imitated structure wood and a preparation method thereof, and belongs to the technical field of structural wood preparation. In order to develop the structural wood which is simple and convenient in preparation method and excellent in performance, poplar veneers are soaked in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, swelling is conducted for 36-40 h at the temperature of 50-55 DEG C, then the poplar veneers are added into maleic anhydride, and esterification modification is conducted at the room temperature for 3-4 h; then rinsing for multiple times, soaking in a sodium hydroxide aqueous solution for 3-4 hours to carry out neutralization reaction, rinsing to be neutral, and freeze-drying to obtain the modified poplar veneer; a mixed aqueous solution of ammonium dihydrogen phosphate and magnesium chloride is prepared, the modified poplar veneer is placed in the mixed aqueous solution to be subjected to vacuum impregnation for 3-4 h, then the modified poplar veneer is transferred into a sodium silicate solution with a certain concentration to be subjected to vacuum impregnation for 3-4 h, and a mineralized poplar veneer is obtained; and shell-imitated structure single-layer poplar is prepared, specifically, the mineralized poplar veneer is subjected to densification treatment, and the shell-imitated structure poplar is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of structural wood preparation, and in particular relates to a high-performance shell-like structural wood and a preparation method thereof. Background Art

[0002] At present, there is a shortage of natural wood resources that can be directly used. The development of fast-growing wood that grows fast, matures early, and has a short rotation period has attracted widespread attention. However, due to the loose texture, low density, and large porosity of fast-growing wood, its mechanical and mechanical strength are unsatisfactory, which seriously limits its application. It is urgent to develop efficient technologies to physically or chemically modify fast-growing wood.

[0003] The invention patent with patent number CN112171830B and invention name "A high-strength wood and its preparation method" discloses the technical solution as "The high-strength wood is a dense microstructure formed by the dense arrangement of wood cell units. The wood cell units are solid structures composed of nanocellulose fibers and lignin. The content of lignin ranges from 0% to 90%. The preparation method of the present invention is: first, through the process of removing lignin, obtain wood with partial lignin removal; then treat the wood fibers with a chemical solution, and finally wash with water to remove chemical residues in the sample, and obtain high-strength wood after drying. The high-strength wood has greatly improved density and mechanics. The preparation method has the characteristics of wide range of raw materials, simple preparation steps, low cost, etc., which greatly expands the application range of wood." However, this method requires delignification of the wood through harsh chemical treatment (sodium hydroxide / sodium sulfite treatment). Summary of the invention

[0004] The problem to be solved by the present invention is to develop a structural wood with a simple preparation method and excellent performance, and to propose a high-performance shell-like structural wood and a preparation method thereof.

[0005] To achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A method for preparing high-performance shell-like structural wood comprises the following steps:

[0007] S1. Poplar veneer modification: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 50-55° C. for 36-40 hours, and then the poplar veneer is added to maleic anhydride and kept at room temperature for 3-4 hours for esterification modification;

[0008] Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 3-4 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer;

[0009] S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 3-4 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 3-4 hours to obtain a mineralized poplar veneer;

[0010] S3. Preparation of single-layer poplar wood with imitation shell structure: densification treatment is performed on the mineralized poplar wood veneer obtained in step S2 to obtain poplar wood with imitation shell structure.

[0011] Furthermore, for the preparation of the shell-like structure multi-layer poplar: a layer of adhesive is coated on the surface of the shell-like structure poplar veneer obtained in step S3, and the veneers coated with adhesive are stacked layer by layer with the fiber directions of two adjacent veneers perpendicular to each other, and hot-pressed to obtain the shell-like structure multi-layer poplar.

[0012] Furthermore, in step S1, the material-liquid ratio of the poplar veneer and the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g: 100-120 mL;

[0013] In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 2-4 mg / mL;

[0014] The mass ratio of the poplar veneer to maleic anhydride is 1:3-5.

[0015] Furthermore, in step S1, the number of ethanol rinsing is 3-5 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 12-48 hours.

[0016] Furthermore, in step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 30-35wt%, the concentration of magnesium chloride in the mixed aqueous solution is 15-20wt%; and the concentration of the sodium silicate solution is 10-50wt%.

[0017] Furthermore, in step S3, the densification treatment conditions are 10-100 MPa and 60-120° C. for 6-8 hours.

[0018] Furthermore, the adhesive coated on the surface during the preparation of the multi-layer poplar wood with imitation shell structure is one of starch adhesive, soybean protein adhesive, isocyanate adhesive, epoxy resin adhesive, polyurethane adhesive, and polyvinyl acetate adhesive.

[0019] Furthermore, the hot pressing treatment conditions in the preparation of the shell-like structure multi-layer poplar wood are 10-100MPa, 60-120℃ and hot pressing for 6-8h.

[0020] A method for preparing high-performance imitation shell structural wood provides a high-performance imitation shell structural wood, wherein the flame retardant property of the high-performance imitation shell structural wood meets the Class B requirement specified in GB / T11785 "Classification of Fire Performance of Artificial Panels" standard.

[0021] Beneficial effects of the present invention:

[0022] The method for preparing a high-performance shell-like structural wood of the present invention comprises pre-treating poplar veneer with a lithium hydroxide / dimethyl sulfoxide solution to enlarge the intercellular space of the wood, and then performing an esterification reaction to enhance the electrostatic repulsion to further enlarge the intercellular space of the wood, thereby enhancing the penetration of inorganic salt modified precursors, and introducing sites for in-situ mineralization of inorganic salts, and finally obtaining a shell-like structural high-performance wood through in-situ inorganic salt mineralization combined with a densification process, which can be used as structural wood in the fields of construction, furniture, interior decoration, etc. .

[0023] The method for preparing a high-performance imitation shell structural wood described in the present invention increases the intercellular space of the wood to enhance the penetration of inorganic salt modified precursors through the cell swelling technology combined with the electrostatic repulsion introduced by esterification, and introduces sites for in-situ mineralization of inorganic salts, and further performs in-situ inorganic salt mineralization and densification, and finally obtains high-performance imitation shell structural wood. This method does not require delignification treatment, and avoids the use of highly toxic chemicals such as formaldehyde, while achieving high performance such as flame retardancy. The tensile strength of the imitation shell structural wood obtained by this method is 2-3 times higher than that of the original poplar veneer, and the compressive strength is increased by 1.5-2 times. At the same time, the flame retardant performance meets the Class B requirements specified in the GB / T11785 "Classification of Fire Performance of Artificial Panels" standard. In addition, the obtained imitation shell structural poplar wood can be bonded together by adhesive bonding to obtain a multi-layer imitation shell structural poplar wood. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic flow chart of a method for preparing a high-performance shell-like structural wood according to the present invention;

[0025] Figure 2 These are photos of samples at various stages in the preparation process of the present invention;

[0026] Figure 3 This is a SEM image of the cross section of poplar wood in the present invention;

[0027] Figure 4 This is a SEM image of the cross section of the modified poplar wood of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the specific embodiments described are only part of the embodiments of the present invention, rather than all of the specific embodiments. The components of the specific embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations, and the present invention can also have other embodiments.

[0029] Therefore, the following detailed description of the specific embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected specific embodiments of the present invention. Based on the specific embodiments of the present invention, all other specific embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0030] In order to further understand the content, features and effects of the present invention, the following specific implementation methods are given as examples, and the attached Figure 1 -Attached Figure 4 The detailed instructions are as follows:

[0031] Embodiment 1:

[0032] A method for preparing high-performance shell-like structural wood comprises the following steps:

[0033] S1. Modification of poplar veneer: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 50°C for 36 hours. Then, the poplar veneer is added to maleic anhydride and kept at room temperature for 3 hours for esterification modification.

[0034] Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 3 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer;

[0035] Furthermore, in step S1, the material-liquid ratio of the poplar veneer and the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g: 100 mL;

[0036] In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 2 mg / mL;

[0037] The mass ratio of the poplar veneer to maleic anhydride is 1:3.

[0038] Furthermore, in step S1, the number of ethanol rinsing is 3 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 24 hours.

[0039] S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 3 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 3 hours to obtain a mineralized poplar veneer;

[0040] Furthermore, in step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 30wt%, the concentration of magnesium chloride in the mixed aqueous solution is 15wt%; and the concentration of the sodium silicate solution is 20wt%.

[0041] S3. Preparation of a single-layer poplar wood with a shell-like structure: The mineralized poplar wood veneer obtained in step S2 is densified to obtain a poplar wood with a shell-like structure;

[0042] Furthermore, in step S3, the densification treatment conditions are 10 MPa and 80° C. for 6 h;

[0043] The high-performance imitation shell structural timber prepared by the preparation method of the high-performance imitation shell structural timber described in this embodiment is characterized in that the flame retardant properties of the high-performance imitation shell structural timber meet the Class B requirements specified in the GB / T11785 "Classification of Fire Resistance of Artificial Panels" standard.

[0044] A high-performance shell-like structural wood prepared in this embodiment, such as Figure 2 As shown, from Figure 2 It can be seen that through the cell swelling process, in-situ mineralization technology, and densification process, a brown-yellow and uniform shell-like structural wood can be obtained; SEM images are compared. Figure 3 and Figure 4 As shown in the figure, a looser wood structure can be obtained through chemical swelling pretreatment, and the cell swelling process can open the dense cell structure of poplar, which facilitates the penetration and in-situ mineralization of subsequent modifiers.

[0045] A high-performance shell-like structural wood prepared in this embodiment has performance tests as shown in Table 1:

[0046] Table 1:

[0047]

[0048] The flame retardant standard is GB / T11785 "Classification of Fire Performance of Artificial Boards". As can be seen from Table 1, the tensile strength of the obtained imitation shell structural wood is 2-3 times higher than that of the original poplar veneer, and the compressive strength is increased by 1.5-2 times. At the same time, the flame retardant performance meets the Class B requirements specified in GB / T11785 "Classification of Fire Performance of Artificial Boards".

[0049] Embodiment 2:

[0050] A method for preparing high-performance shell-like structural wood comprises the following steps:

[0051] S1. Modification of poplar veneer: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 55°C for 40 hours. Then, the poplar veneer is added to maleic anhydride and kept at room temperature for 4 hours for esterification modification;

[0052] Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 4 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer;

[0053] Furthermore, in step S1, the material-liquid ratio of the poplar veneer to the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g:120 mL;

[0054] In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 4 mg / mL;

[0055] The mass ratio of the poplar veneer to maleic anhydride is 1:5.

[0056] Furthermore, in step S1, the number of ethanol rinsing is 5 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 12 hours.

[0057] S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 4 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 4 hours to obtain a mineralized poplar veneer;

[0058] Furthermore, in step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 35wt%, the concentration of magnesium chloride in the mixed aqueous solution is 20wt%; and the concentration of the sodium silicate solution is 50wt%.

[0059] S3. Preparation of a single-layer poplar wood with a shell-like structure: The mineralized poplar wood veneer obtained in step S2 is densified to obtain a poplar wood with a shell-like structure;

[0060] Furthermore, in step S3, the densification treatment conditions are 100 MPa and 120° C. for 8 h;

[0061] S4. Preparation of multilayer poplar wood with shell-like structure: A layer of adhesive is applied to the surface of the poplar wood veneer with shell-like structure obtained in step S3, and the veneers coated with adhesive are stacked layer by layer in such a way that the fiber directions of two adjacent veneers are perpendicular to each other, and the multilayer poplar wood with shell-like structure is obtained by hot pressing;

[0062] Furthermore, the adhesive coated on the surface in step S4 is a soy protein adhesive;

[0063] Furthermore, in step S4, the hot pressing treatment conditions are 50 MPa and 60° C. for 6 hours.

[0064] The high-performance imitation shell structural timber prepared by the preparation method of the high-performance imitation shell structural timber described in this embodiment is characterized in that the flame retardant properties of the high-performance imitation shell structural timber meet the Class B requirements specified in the GB / T11785 "Classification of Fire Resistance of Artificial Panels" standard.

[0065] Embodiment 3:

[0066] A method for preparing high-performance shell-like structural wood comprises the following steps:

[0067] S1. Modification of poplar veneer: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 55°C for 36 hours. Then, the poplar veneer is added to maleic anhydride and kept at room temperature for 4 hours for esterification modification;

[0068] Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 4 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer;

[0069] Furthermore, in step S1, the material-liquid ratio of the poplar veneer to the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g:110 mL;

[0070] In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 3 mg / mL;

[0071] The mass ratio of the poplar veneer to maleic anhydride is 1:4.

[0072] Furthermore, in step S1, the number of ethanol rinsing is 4 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 48 hours.

[0073] S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 3 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 3 hours to obtain a mineralized poplar veneer;

[0074] Furthermore, in step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 32wt%, the concentration of magnesium chloride in the mixed aqueous solution is 16wt%; and the concentration of the sodium silicate solution is 25wt%.

[0075] S3. Preparation of a single-layer poplar wood with a shell-like structure: The mineralized poplar wood veneer obtained in step S2 is densified to obtain a poplar wood with a shell-like structure;

[0076] Furthermore, in step S3, the densification treatment conditions are 20MPa, 60-120°C for 7h;

[0077] The high-performance imitation shell structural timber prepared by the preparation method of the high-performance imitation shell structural timber described in this embodiment is characterized in that the flame retardant properties of the high-performance imitation shell structural timber meet the Class B requirements specified in the GB / T11785 "Classification of Fire Resistance of Artificial Panels" standard.

[0078] Embodiment 4:

[0079] A method for preparing high-performance shell-like structural wood comprises the following steps:

[0080] S1. Modification of poplar veneer: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 50°C for 36 hours. Then, the poplar veneer is added to maleic anhydride and kept at room temperature for 3-4 hours for esterification modification;

[0081] Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 3.5 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer;

[0082] Furthermore, in step S1, the material-liquid ratio of the poplar veneer and the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g: 100 mL;

[0083] In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 3 mg / mL;

[0084] The mass ratio of the poplar veneer to maleic anhydride is 1:3.5.

[0085] Furthermore, in step S1, the number of ethanol rinsing is 5 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 12-48 hours.

[0086] S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 3 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 3 hours to obtain a mineralized poplar veneer;

[0087] Furthermore, in step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 33wt%, the concentration of magnesium chloride in the mixed aqueous solution is 17wt%; and the concentration of the sodium silicate solution is 30wt%.

[0088] S3. Preparation of a single-layer poplar wood with a shell-like structure: The mineralized poplar wood veneer obtained in step S2 is densified to obtain a poplar wood with a shell-like structure;

[0089] Furthermore, in step S3, the densification treatment conditions are 50 MPa and 100° C. for 6 h;

[0090] S4. Preparation of multilayer poplar wood with shell-like structure: A layer of adhesive is applied to the surface of the poplar wood veneer with shell-like structure obtained in step S3, and the veneers coated with adhesive are stacked layer by layer in such a way that the fiber directions of two adjacent veneers are perpendicular to each other, and the multilayer poplar wood with shell-like structure is obtained by hot pressing;

[0091] Furthermore, the adhesive applied to the surface in step S4 is an isocyanate adhesive;

[0092] Furthermore, in step S4, the hot pressing treatment conditions are 20 MPa and 120° C. for 6 hours.

[0093] The high-performance imitation shell structural timber prepared by the preparation method of the high-performance imitation shell structural timber described in this embodiment is characterized in that the flame retardant properties of the high-performance imitation shell structural timber meet the Class B requirements specified in the GB / T11785 "Classification of Fire Resistance of Artificial Panels" standard.

[0094] Embodiment 5:

[0095] A method for preparing high-performance shell-like structural wood comprises the following steps:

[0096] S1. Poplar veneer modification: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 50°C for 39 hours. Then, the poplar veneer is added to maleic anhydride and kept at room temperature for 3 hours for esterification modification;

[0097] Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 3 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer;

[0098] Furthermore, in step S1, the material-liquid ratio of the poplar veneer to the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g:120 mL;

[0099] In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 4 mg / mL;

[0100] The mass ratio of the poplar veneer to maleic anhydride is 1:3.

[0101] Furthermore, in step S1, the number of ethanol rinsing is 4 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 48 hours.

[0102] S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 3 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 3 hours to obtain a mineralized poplar veneer;

[0103] Furthermore, in step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 30wt%, the concentration of magnesium chloride in the mixed aqueous solution is 15wt%; and the concentration of the sodium silicate solution is 40wt%.

[0104] S3. Preparation of a single-layer poplar wood with a shell-like structure: The mineralized poplar wood veneer obtained in step S2 is densified to obtain a poplar wood with a shell-like structure;

[0105] Furthermore, in step S3, the densification treatment conditions are 30 MPa and 90° C. for 8 h;

[0106] S4. Preparation of multilayer poplar wood with shell-like structure: A layer of adhesive is applied to the surface of the poplar wood veneer with shell-like structure obtained in step S3, and the veneers coated with adhesive are stacked layer by layer in such a way that the fiber directions of two adjacent veneers are perpendicular to each other, and the multilayer poplar wood with shell-like structure is obtained by hot pressing;

[0107] Furthermore, the adhesive coated on the surface in step S4 is a polyvinyl acetate adhesive;

[0108] Furthermore, in step S4, the hot pressing treatment conditions are 10 MPa and 60° C. for 8 hours.

[0109] The high-performance imitation shell structural timber prepared by the preparation method of the high-performance imitation shell structural timber described in this embodiment is characterized in that the flame retardant properties of the high-performance imitation shell structural timber meet the Class B requirements specified in the GB / T11785 "Classification of Fire Resistance of Artificial Panels" standard.

[0110] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0111] Although the present application has been described above with reference to specific embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, as long as there is no structural conflict, the various features in the specific embodiments disclosed in the present application may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for preparing high-performance shell-like structural wood, characterized in that: The steps include: S1. Poplar veneer modification: First, the poplar veneer is immersed in a mixed solution of lithium hydroxide and dimethyl sulfoxide according to the material-liquid ratio, and swells at 50-55° C. for 36-40 hours, and then the poplar veneer is added to maleic anhydride and kept at room temperature for 3-4 hours for esterification modification; Then, the poplar veneer is taken out from the maleic anhydride, rinsed with an ethanol solution for multiple times, and then immersed in a sodium hydroxide aqueous solution for 3-4 hours for neutralization reaction, and then rinsed with distilled water until neutral, and then freeze-dried to obtain a modified poplar veneer; S2. Mineralization of poplar veneer: a certain concentration of ammonium dihydrogen phosphate and magnesium chloride mixed aqueous solution is prepared, the modified poplar veneer obtained in step S1 is placed in the mixed aqueous solution for vacuum impregnation for 3-4 hours, and then transferred to a certain concentration of sodium silicate solution for vacuum impregnation for 3-4 hours to obtain a mineralized poplar veneer; S3. Preparation of single-layer poplar wood with imitation shell structure: densification treatment is performed on the mineralized poplar wood veneer obtained in step S2 to obtain poplar wood with imitation shell structure.

2. The method for preparing a high-performance shell-like structural timber according to claim 1, characterized in that: Preparation of multi-layer poplar wood with imitation shell structure: a layer of adhesive is coated on the surface of the poplar wood veneer with imitation shell structure obtained in step S3, and the veneers coated with adhesive are stacked layer by layer with the fiber directions of two adjacent veneers perpendicular to each other, and hot-pressed to obtain the multi-layer poplar wood with imitation shell structure.

3. The method for preparing a high-performance shell-like structural timber according to claim 1 or 2, characterized in that: In step S1, the material-liquid ratio of the poplar veneer to the mixed solution of lithium hydroxide and dimethyl sulfoxide is 1 g: 100-120 mL; In the mixed solution of lithium hydroxide and dimethyl sulfoxide, the concentration of lithium hydroxide is 2-4 mg / mL; The mass ratio of the poplar veneer to maleic anhydride is 1:3-5.

4. The method for preparing a high-performance shell-like structural timber according to claim 3, characterized in that: In step S1, the number of ethanol rinsing is 3-5 times, the pH of the sodium hydroxide aqueous solution is 10, the freeze-drying conditions are 1 Pa, -50°C, and the freeze-drying time is 12-48 hours.

5. The method for preparing a high-performance shell-like structural timber according to claim 4, characterized in that: In step S2, the concentration of ammonium dihydrogen phosphate in the mixed aqueous solution is 30-35wt%, the concentration of magnesium chloride in the mixed aqueous solution is 15-20wt%; and the concentration of the sodium silicate solution is 10-50wt%.

6. The method for preparing a high-performance shell-like structural timber according to claim 5, characterized in that: The densification treatment conditions in step S3 are 10-100 MPa, 60-120° C., and densification for 6-8 hours.

7. The method for preparing high-performance shell-like structural timber according to claim 6, characterized in that: The adhesive coated on the surface during the preparation of the multi-layer poplar wood with imitation shell structure is one of starch adhesive, soybean protein adhesive, isocyanate adhesive, epoxy resin adhesive, polyurethane adhesive and polyvinyl acetate adhesive.

8. The method for preparing high-performance shell-like structural timber according to claim 7, characterized in that: The hot pressing treatment conditions in the preparation of the shell-like structure multi-layer poplar are 10-100MPa, 60-120℃ and hot pressing for 6-8h.

9. A high-performance imitation shell structural timber prepared by the method for preparing a high-performance imitation shell structural timber according to any one of claims 1 to 8, characterized in that: The flame retardant properties of the high-performance imitation shell structural wood meet the Class B requirements specified in the GB / T11785 "Classification of Fire Resistance of Artificial Panels" standard.

Citation Information

Patent Citations

  • Composite material having shell nacre-imitated layered structure as well as preparation method and application of composite material

    CN105774182A

  • Composite flame retardant and waterproof modifying agent for modification of fast-growing wood for manufacturing outdoor furniture

    CN106363738A

  • Multifunctional treating method for planted fast-growing forest wood

    CN106426451A

  • Anti-flame large-breadth width-splicing dipping decoration veneer and manufacturing method thereof

    CN108858529A

  • Complexing single plate, complexing single plate composite material and manufacturing methods thereof

    CN110480764A

Cited By

  • Wear-resistant and compression-resistant laminated bamboo plywood and preparation method thereof

    CN120552160A

  • Wear-resistant and pressure-resistant laminated bamboo plywood and preparation method thereof

    CN120552160B