Method for forming groove and semiconductor process equipment
Through the alternating cycle etching method, the mutual cancellation effect of the first etching step and the second etching step is used to solve the problem of rounded corners and micro-grooves at the bottom of the trench in the dry etching process, and realize the bottom of the trench. The flatness improves the preparation quality and process efficiency of semiconductor structures.
Patent Information
- Application Number
- CN202410749484.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
AI Technical Summary
When forming deep silicon trenches using the existing dry etching process, it is easy to form rounded corners or micro-grooves at the bottom of the trench, which affects the preparation of subsequent semiconductor structures, and is especially unfavorable for the manufacturing of MEMS and buried fan-out packaging structures. .
Using an alternating cycle etching method, the bottom fillet and micro-groove effects generated by the first etching step and the second etching step offset each other to ensure that the bottom of the trench is flat. The specific method includes performing a first etching step and a second etching step in each cycle. The first etching step produces a bottom fillet, and the second etching step produces a micro-groove effect, and by controlling the deposition step, physical bombardment Steps and process conditions for chemical etching steps, optimizing the etching process to eliminate fillets and micro-grooves.
The flattening of the trench bottom is achieved, which improves the preparation conditions of subsequent semiconductor structures, especially the quality of MEMS and buried fan-out packaging structures, simplifies process steps and reduces processing costs.
Smart Images

Figure CN118771302A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a groove and a semiconductor process equipment. Background Art
[0002] In the fields of integrated circuits, micro-electromechanical systems, and advanced packaging, deep silicon etching has important applications and is a very important process in semiconductor manufacturing. Since deep silicon etching requires the formation of grooves with a large aspect ratio and high verticality, the traditional wet etching process cannot be completed, so a dry etching process is usually used to obtain the required grooves. Among them, the dry etching process is an etching technology based on low-temperature plasma, which uses ionized gas to physically bombard and chemically etch the film layer to be etched to achieve the etching purpose. However, because the isotropic etching effect of chemical etching or the anisotropic effect of physical bombardment easily leads to the formation of fillets or micro-grooves at the bottom of the groove, this will be detrimental to the subsequent preparation of semiconductor structures, such as the preparation of MEMS (full name Micro Electro Mechanical System) structures or buried fan-out packaging structures. Summary of the invention
[0003] The present application provides a method for forming a groove and a semiconductor process equipment to solve the problem in the related art that the bottom of the groove is prone to form a rounded corner or a micro groove, which is not conducive to the subsequent preparation of a semiconductor structure.
[0004] A first aspect of the present application provides a method for forming a groove, which is applied to a film layer to be etched, wherein the film layer to be etched includes a stacked substrate and a mask layer, wherein the mask layer is provided with a first mask opening, and the method includes: alternately performing a first etching step and a second etching step in a cycle to form a first groove in the substrate; wherein, in each round of the total cycle, the first etching step is used to etch a first portion of the substrate exposed from the first mask opening to a first predetermined depth, and the second etching step is used to etch a first portion of the substrate exposed from the first mask opening to a second predetermined depth; and, in each round of the total cycle, one of the first etching step and the second etching step produces a bottom fillet, and the other of the first etching step and the second etching step produces a micro-groove effect.
[0005] In one embodiment, the mask layer is further provided with a second mask opening, the second mask opening exposes a second portion of the substrate, and the opening size of the second mask opening is smaller than the opening size of the first mask opening; the method further comprises: in the process of performing the first etching step and the second etching step in an alternating cycle, a second groove is also formed in the substrate; wherein, in each total cycle, in the etching step for producing the bottom fillet, the etching rate for the first portion is greater than the etching rate for the second portion, and in the etching step for producing the micro-groove effect, the etching rate for the first portion is less than the etching rate for the second portion.
[0006] In one embodiment, in each total cycle, the second portion is etched to a third predetermined depth, and the third predetermined depth is equal to or greater than the sum of the first predetermined depth and the second predetermined depth.
[0007] In one embodiment, the second etching step is an etching step for producing a micro-groove effect, and the second etching step includes a main etching step. The process conditions of the main etching step include: the upper electrode center power and the upper electrode edge power are both in the range of 100W to 500W.
[0008] In one embodiment, at least one of the upper electrode center power and the upper electrode edge power is less than 200W.
[0009] In one embodiment, the second etching step further includes a pre-etching step, which is performed before the main etching step; the pre-etching step is used to remove etching by-products formed in the first etching step.
[0010] In one embodiment, the material of the substrate is a silicon-containing material, the process conditions of the pre-etching step include the etching gas being a carbon-containing or fluorine-containing gas, and the process conditions of the main etching step include the etching gas being a sulfur-containing or fluorine-containing gas.
[0011] In one embodiment, the first etching step is an etching step for producing a bottom fillet, and the first etching step includes a sub-cycle of cyclically executing a deposition step, a physical bombardment step, and a chemical etching step; wherein, in each round of the sub-cycle, the deposition step, the physical bombardment step, and the chemical etching step are sequentially executed; in all the rounds of the sub-cycle, the method further includes at least one of the following:
[0012] The deposition time of the deposition step increases in sequence according to the number of cycles of the sub-cycle;
[0013] The power of the lower electrode in the physical bombardment step increases in sequence according to the number of cycles of the sub-cycle;
[0014] The etching time of the chemical etching step decreases in sequence according to the number of sub-cycles.
[0015] In one embodiment, in all rounds of the total cycle, the method further includes at least one of the following:
[0016] The increment of the deposition time increases in sequence according to the number of cycles of the total cycle;
[0017] The increment of the lower electrode power in the physical bombardment step increases in sequence according to the number of cycles of the total cycle;
[0018] The increment of etching time of the chemical etching step decreases in sequence according to the number of cycles of the total cycle.
[0019] In one embodiment, in the nth round cycle, at least one of the deposition time t1, the lower electrode power P and the etching time t2 satisfies the following relationship:
[0020]
[0021] Among them, t1 init is the initial deposition time, t1 final is the target deposition time, N total is the total number of sub-cycles, M total is the total number of rounds in the total cycle, P init is the initial lower electrode power, P final is the target lower electrode power, t2 init is the initial etching time, t2 final is the target etching time, n, N total and M total All are positive integers.
[0022] In one embodiment, the first trench is used as a cavity of a MEMS structure or as a chip receiving cavity of a buried fan-out packaging structure.
[0023] The second aspect of the present application provides a semiconductor process equipment, including a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, the controller including at least one processor and at least one memory, the memory storing a computer program, and when the computer program is executed by the processor, a method of any of the above-mentioned embodiments is implemented.
[0024] The advantages or beneficial effects of the above technical solution include at least: in the process of forming the first groove, by alternately executing the first etching step and the second etching step in a cycle, the first etching step can be executed first in each cycle to etch the first part of the substrate exposed from the first mask opening to a first predetermined depth, and then the second etching step is executed to continue etching the first part of the substrate exposed from the first mask opening to a second predetermined depth, and one of the first etching step and the second etching step produces a bottom fillet, and the other of the first etching step and the second etching step produces a micro-groove effect, so that the generated micro-groove effect and the generated bottom fillet can be offset during the etching process, so that the bottom fillet or micro-groove generated by executing the first etching step in each cycle can be eliminated, thereby ensuring that the bottom of the first groove finally obtained is flat, which is beneficial to the subsequent preparation of semiconductor structures, such as the subsequent preparation of MEMS structures and buried fan-out packaging structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings herein are incorporated into and constitute a part of the specification, illustrate embodiments consistent with the present application, and together with the specification are used to explain the principles of the present application. In addition, these drawings and text descriptions are not intended to limit the scope of the concept of the present application in any way, but to illustrate the concept of the present application for those skilled in the art by referring to specific embodiments.
[0026] Figure 1A The schematic diagram shown is a chip placed in the first trench with a flat bottom.
[0027] Figure 1B The schematic diagram shows a chip placed in a first trench with rounded bottom.
[0028] Figure 2 FIG. 1 is a schematic flow chart of a method for forming a trench according to an embodiment of the present application.
[0029] FIG. 3A to FIG. 3D Shown is a schematic cross-sectional structure diagram of each step in a method for forming a groove according to an embodiment of the present application.
[0030] Figure 3E Shown Figure 3D Schematic diagram of the electron microscope at the left corner of the bottom of the first trench.
[0031] Figure 4 The figure is a schematic diagram showing the effect of the loading effect produced by executing the second etching step alone.
[0032] Figure 5 FIG. 4 is a schematic flow chart of a method for forming a groove according to another embodiment of the present application.
[0033] Fig. 6A FIG. 1 is a schematic electron microscope diagram of forming the first sub-groove in the first example.
[0034] Figure 6B Shown Fig. 6A Schematic diagram of the electron microscope at the left corner of the bottom of the first sub-trench.
[0035] Figure 6C FIG. 4 is a schematic electron microscope diagram of forming the second sub-trench in the first example.
[0036] Fig. 7A Shown is a schematic electron microscope diagram of forming the first sub-trench in the second example.
[0037] Figure 7B FIG. 4 is a schematic diagram of an electron microscope for forming a second sub-trench in the second example.
[0038] FIG. 8A to FIG. 8D Shown is a schematic cross-sectional structure diagram of each step in the process of forming a cavity of a MEMS structure using the method of an embodiment of the present application.
[0039] FIG. 9A to FIG. 9G Shown is a schematic cross-sectional structure diagram of each step in a process of forming a buried fan-out packaging structure using the method of an embodiment of the present application.
[0040] Fig.10 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application. DETAILED DESCRIPTION
[0041] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0042] In practical applications, the MEMS structure and the embedded fan-out packaging structure usually need to form a first trench with a large opening size and a flat bottom in the substrate. The first trench can be used as a cavity in the MEMS structure or as a chip accommodating cavity in the embedded fan-out packaging structure. Take the first trench in the substrate as the chip accommodating cavity of the embedded fan-out packaging structure as an example. Figure 1A As shown, when the bottom of the first groove 111 is flat, the chip 30 can be normally placed in the first groove 111; when the bottom of the first groove 111 has rounded corners or micro grooves, as shown in FIG. Figure 1BAs shown, when the bottom of the first groove 111 has a rounded corner, for example, the chip 30 is easily tilted during the process of being placed in the first groove 111, which has an adverse effect on the placement of the chip 30. However, in the related art, since the dry etching process is accompanied by chemical etching and physical bombardment, the isotropic effect of chemical etching easily leads to the formation of a rounded corner at the bottom of the first groove 111, and the anisotropic effect of physical bombardment easily leads to the formation of a micro groove at the bottom of the first groove 111, which is not conducive to the subsequent preparation of a MEMS structure or an embedded fan-out packaging structure.
[0043] In view of this, the embodiment of the present application provides a method for forming a groove and a semiconductor process equipment to solve the problem that the bottom of the first groove is prone to form a rounded corner or a micro groove, which is not conducive to the subsequent preparation of the semiconductor structure. The technical solution of the embodiment of the present application is described in detail below with reference to the accompanying drawings.
[0044] Figure 2 FIG. 1 is a schematic flow chart of a method for forming a trench according to an embodiment of the present application. FIG. 3A to FIG. 3D Shown is a schematic cross-sectional structure diagram of each step in a method for forming a groove according to an embodiment of the present application. Figure 3E Shown Figure 3D Schematic diagram of the electron microscope structure at the left corner of the bottom of the first trench.
[0045] Please also read Figure 2 , FIG. 3A to FIG. 3D , the method for forming a groove can be applied to a film layer 10 to be etched, wherein the film layer 10 to be etched includes a stacked substrate 11 and a mask layer 12, wherein the mask layer 12 is provided with a first mask opening 12A. The method for forming a groove includes: alternately performing a first etching step and a second etching step in a cycle to form a first groove 111 in the substrate 11. In each round of the total cycle, the first etching step is used to etch the first portion of the substrate 11 exposed from the first mask opening 12A to a first predetermined depth h11, and the second etching step is used to etch the first portion of the substrate 11 exposed from the first mask opening 12A to a second predetermined depth h12; and in each round of the total cycle, one of the first etching step and the second etching step generates a bottom fillet, and the other of the first etching step and the second etching step generates a sub-trench effect, so as to eliminate the bottom fillet by using the sub-trench effect, or to eliminate the sub-trench effect by using the bottom fillet. Among them, one total cycle is to perform one round of the first etching step and the second etching step in an alternating cycle.
[0046] It should be noted that the micro-groove effect refers to the phenomenon that during the etching process, the etching rate at the bottom corners of the groove is greater than the etching rate at the center of the groove. This phenomenon is caused by the fact that when high-energy plasma bombards the sidewalls of the groove at a certain angle, the energy of the plasma is not completely consumed and is reflected by the sidewalls of the groove and slides down to the bottom corners of the groove, which increases the etching rate at the bottom corners of the groove, resulting in the etching rate at the bottom corners of the groove being greater than the etching rate at the center of the groove. For example, Figure 4 As shown, taking a single etching step for generating the micro-groove effect as an example, the micro-groove effect will cause micro-grooves 1111B to be formed at the bottom corners of the first sub-groove 1111 formed in the substrate 11 .
[0047] For example, Figure 2 As shown, in each cycle, the method for forming a groove may include the following steps S110 to S120.
[0048] Step S110, please refer to FIG. 3A to FIG. 3B , performing a first etching step to etch the first portion of the substrate 11 exposed from the first mask opening 12A to a first predetermined depth h11.
[0049] Step S120, please refer to FIG. 3B to FIG. 3C , perform a second etching step to etch the first portion of the substrate 11 exposed from the first mask opening 12A to a second predetermined depth h12; wherein one of the first etching step and the second etching step produces a bottom fillet, and the other of the first etching step and the second etching step produces a micro-groove effect.
[0050] For example, in the first round of alternating cycles, the first etching step and the second etching step are performed, and the first etching step is an etching step for generating a bottom fillet, and the second etching step is an etching step for generating a micro-groove effect. FIG. 3A to FIG. 3B As shown, after the first etching step is performed, the first portion of the substrate 11 exposed from the first mask opening 12A is etched to a first predetermined depth h11, and a first sub-groove 1111 having a rounded corner 1111A at the bottom corner is formed in the substrate 11; FIG. 3B to FIG. 3C In the process of performing the second etching step, the first portion is continuously etched and a micro-groove effect is generated, so that the first portion can be continuously etched to the second predetermined depth h12, increasing the etching depth of the first sub-groove 1111, and the bottom fillet 1111A of the first sub-groove 1111 can be eliminated during the etching process to ensure that the bottom of the first sub-groove 1111 is flat. Based on this, by alternately performing the first etching step and the second etching step for a preset total number of rounds, a first groove 111 with a flat bottom (such as Figure 3D ), for example, from Figure 3EThe local electron microscope schematic diagram shows that the left corner of the bottom of the first groove 111 is flat, and no bottom rounded corner is generated. Among them, the first sub-groove 1111 is the intermediate morphology of the first groove 111 during the etching process. After the first etching step and the second etching step are alternately cycled for a preset total number of rounds, the first sub-groove 1111 constitutes the first groove 111.
[0051] For example, please also refer to Figure 4 The first etching step may be an etching step for producing a micro-groove effect, and the second etching step may be an etching step for producing a bottom rounded corner. By alternately and cyclically executing the first etching step and the second etching step for a preset total number of rounds, the micro-groove 1111B of the first sub-groove 1111 can be eliminated during the etching process, thereby ensuring that the bottom of the first sub-groove 1111 is flat.
[0052] In the above scheme, in the process of forming the first groove 111, the first etching step and the second etching step are performed alternately and cyclically. In each cycle, the first etching step can be performed first to etch the first portion of the substrate 11 exposed from the first mask opening 12A to a first predetermined depth h11, and then the second etching step can be performed to continue etching the first portion of the substrate 11 exposed from the first mask opening 12A to a second predetermined depth h12, and one of the first etching step and the second etching step produces a bottom fillet, and the other of the first etching step and the second etching step produces a micro-groove effect, so that the generated micro-groove effect and the generated bottom fillet can be offset each other during the etching process, so that the bottom fillet 1111A or the micro-groove 1111B generated by the first etching step in each cycle can be eliminated, thereby ensuring that the bottom of the first groove 111 finally obtained is flat, which is beneficial to the subsequent preparation of semiconductor structures, such as the subsequent preparation of MEMS structures and buried fan-out packaging structures.
[0053] It should be noted that, in the process of etching, there is usually an aspect ratio effect (ARDE) or a loading effect. Among them, the aspect ratio effect is that as the etching depth increases, the difficulty of etching reactants such as plasma entering the bottom of the groove increases, and the difficulty of extracting etching byproducts from the bottom of the groove also increases, so that the etching rate of the groove with a large opening size is faster than the etching rate of the groove with a small opening size, resulting in the etching depth of the groove with a large opening size being deeper than the etching depth of the groove with a small opening size. The loading effect is that the rate at which the groove with a large opening size consumes etching reactants such as plasma is faster than the rate at which the groove with a small opening size consumes etching reactants, so that the etching reactants of the groove with a large opening size are insufficient, and the etching rate of the groove with a large opening size is slower than the etching rate of the groove with a small opening size, resulting in the etching depth of the groove with a large opening size finally obtained being shallower than the etching depth of the groove with a small opening size.
[0054] In the related art, since there is usually an aspect ratio effect in the process of etching the first trench 111, in order to eliminate the influence of the aspect ratio effect on the etching depth, please refer to Figure 3A and Figure 3D Usually, the first portion of the substrate 11 exposed from the first mask opening 12A is etched separately to form the first groove 111, and then the second portion of the substrate 11 exposed from the second mask opening 12B is etched separately to form the second groove 112. The first groove 111 and the second groove 112 need to be etched twice separately and cannot be formed by etching at the same time, resulting in the problem of complex process steps and high processing cost in the related technology.
[0055] In order to solve the above technical problems at the same time, FIG. 3A to FIG. 3D As shown, the mask layer 12 is further provided with a second mask opening 12B, the second mask opening 12B exposes the second portion of the substrate 11, and the opening size of the second mask opening 12B is smaller than the opening size of the first mask opening 12A. The opening size is specifically the opening width.
[0056] Please also read FIG. 3A to FIG. 3DThe method for forming a groove further includes: in the process of performing the first etching step and the second etching step in an alternating cycle, forming a second groove 112 in the substrate 11. In each total cycle, in the etching step of generating the bottom fillet, the etching rate of the first portion of the substrate 11 exposed from the first mask opening 12A is greater than the etching rate of the second portion of the substrate 11 exposed from the second mask opening 12B, and in the etching step of generating the micro-groove effect, the etching rate of the first portion is less than the etching rate of the second portion, so that the second portion is etched to a third predetermined depth h13, and the third predetermined depth h13 is equal to or greater than the sum of the first predetermined depth h11 and the second predetermined depth h12.
[0057] Continue to take the first round of alternating cycles to perform the first etching step and the second etching step, and the first etching step is an etching step for generating a bottom fillet, and the second etching step is an etching step for generating a micro-groove effect as an example. FIG. 3A to FIG. 3B As shown, during the first etching step, the etching rate of the first portion of the substrate 11 exposed from the first mask opening 12A is greater than the etching rate of the second portion of the substrate 11 exposed from the second mask opening 12B. Thus, after the first etching step is completed, the etching depth of the first sub-groove 1111 (i.e., the first predetermined depth h11) is deeper than the etching depth of the second sub-groove 1112; wherein the second sub-groove 1112 is an intermediate morphology of the second groove 112 during the etching process. FIG. 3B to FIG. 3C As shown, during the second etching step, the etching rate of the first part of the substrate 11 is less than the etching rate of the second part of the substrate 11. Then, when the second etching step is completed, the etching depth of the second sub-groove 1112 (i.e., the third predetermined depth h13) is equal to or greater than the etching depth of the first sub-groove 1111 (i.e., the sum of the first predetermined depth h11 and the second predetermined depth h12).
[0058] In the above scheme, for each total cycle, during the etching step for producing the bottom fillet, the etching rate of the first portion of the substrate 11 exposed from the first mask opening 12A is controlled to be greater than the etching rate of the second portion of the substrate 11 exposed from the second mask opening 12B, so as to produce an aspect ratio effect, which can make the etching depth of the first portion (that is, the first predetermined depth h11) deeper than the etching depth of the second portion, and during the etching step for producing the micro-groove effect, the loading effect is produced by controlling the etching rate of the first portion of the substrate 11 exposed from the first mask opening 12A to be less than the etching rate of the second portion of the substrate 11 exposed from the second mask opening 12B, so as to make the etching depth of the first portion (that is, the second predetermined depth h12) shallower than the etching depth of the second portion. In this way, after each round of the total cycle is executed, it is helpful to ensure that the etching depth of the second part of the substrate 11 is the same as the etching depth of the first part, that is, the third predetermined depth h13 is equal to or greater than the sum of the first predetermined depth h11 and the second predetermined depth h12. Based on this, by alternately performing the first etching step and the second etching step, the aspect ratio effect and the load effect can be alternately generated in the process of forming the first groove 111 and the second groove 112, and the load effect and the aspect ratio effect are used to counteract each other to achieve the purpose of eliminating the aspect ratio effect, so as to simultaneously form the first groove 111 with a large opening size and a smaller etching depth ha and the second groove 112 with a small opening size and a larger etching depth hb on the substrate 11, thereby simplifying the process steps and reducing the processing cost.
[0059] In one embodiment, Figure 5 As shown, the second etching step is an etching step for producing a micro-groove effect. The second etching step includes a main etching step. The process conditions of the main etching step include: the range of the upper electrode center power and the upper electrode edge power are both 100W to 500W (including the endpoint values).
[0060] During the etching process, the upper electrode power is used to control the ionization rate of the plasma. The size of the upper electrode power is directly proportional to the ionization rate of the plasma. Specifically, the greater the upper electrode power, the higher the ionization rate of the plasma and the higher the plasma content; the smaller the upper electrode power, the lower the ionization rate of the plasma and the lower the plasma content. When the plasma content is low, the substrate 11 exposed by the first mask opening 12A will be etched slowly due to insufficient plasma content, so that the etching rate of the substrate 11 exposed by the first mask opening 12A is lower than the etching rate of the substrate 11 exposed by the second mask opening 12B, which is more likely to produce a load effect instead of an aspect ratio effect.
[0061] Based on this, in the above scheme, in the second etching step, by setting the range of the upper electrode center power and the upper electrode edge power in the main etching step to be between 100W and 500W, the load effect generated in the second etching step can be controlled to antagonize the aspect ratio effect generated in the first etching step, ensuring that after each total cycle, the third predetermined depth h13 of etching the substrate 11 exposed from the second mask opening 12B is greater than the sum of the first predetermined depth h11 and the second predetermined depth h12 of etching the substrate 11 exposed from the first mask opening 12A, ensuring that the etching depth of the second groove 112 finally formed is deeper than the etching depth of the first groove 111.
[0062] In one embodiment, at least one of the upper electrode center power and the upper electrode edge power is less than 200W.
[0063] In one example, the upper electrode power may be 600W, the distribution ratio of the upper electrode center power may be 80%, and the distribution ratio of the upper electrode edge power may be 20%, then the upper electrode center power is equal to 480W, and the upper electrode edge power is equal to 120W.
[0064] In another example, the upper electrode power may be 352W, the distribution ratio of the upper electrode center power may be 55%, and the distribution ratio of the upper electrode edge power may be 45%, then the upper electrode center power is equal to 192.5W, and the upper electrode edge power is equal to 157.5W.
[0065] The above scheme, by configuring at least one of the upper electrode center power and the upper electrode edge power to be less than 200W, can ensure that the upper electrode power is small enough so that the plasma ionization rate is low enough to only generate a small amount of plasma, thereby ensuring that a load effect is generated during the second etching step.
[0066] In one embodiment, Figure 5 As shown, the second etching step also includes a pre-etching step, which is performed before the main etching step; the pre-etching step is used to remove the etching byproducts formed in the first etching step. For example, the first etching step includes: step S121, first performing the pre-etching step; step S122, then performing the main etching step.
[0067] For example, please refer to FIG. 3A to FIG. 3DThe material of the substrate 11 may be a silicon-containing material. The process conditions of the pre-etching step include that the etching gas includes a carbon-containing fluorine-containing gas. The process conditions of the main etching step include that the etching gas includes a sulfur-containing fluorine-containing gas and oxygen. Among them, the carbon-containing fluorine-containing gas has a strong etching effect on silicon oxide. The sulfur-containing fluorine-containing gas has a strong etching effect on silicon. Oxygen can form a silicon-oxygen complex on the sidewalls of the first trench 111 and the second trench 112 during the etching process, thereby protecting the sidewalls of the first trench 111 and the second trench 112 from being etched, so that anisotropic etching can be formed all the way downward.
[0068] In one application scenario, when oxygen is used as an auxiliary gas in the first etching step, silicon oxide (SiO2) is usually formed at the bottom of the first sub-groove 1111 and the bottom of the second sub-groove 1112, and the silicon oxide constitutes an etching byproduct formed in the first etching step. Performing a pre-etching step before performing the main etching step can remove the silicon oxide at the bottom of the first sub-groove 1111 and the second sub-groove 1112, which is conducive to improving the etching efficiency.
[0069] In another application scenario, the material of the mask layer 12 can be photoresist, and the second etching step can also be performed before the first etching step. The carbon-containing and fluorine-containing gases selected for the first round of pre-etching step can also be used to remove the photoresist remaining on the etched surface of the substrate 11 after the mask layer 12 is photolithographically developed, and to remove the native oxide layer on the exposed surfaces of the first and second parts of the substrate 11.
[0070] Optionally, the etching gas in the pre-etching step may be at least one of carbon tetrafluoride (CF4) and trifluoromethane (CHF3). The etching gas in the main etching step may be sulfur hexafluoride (SF6).
[0071] Next, two examples are used to illustrate the effect of sequentially performing the pre-etching step and the main etching step in the present application.
[0072] Table 1 Process parameters of each step of the second etching step in the first example
[0073]
[0074] Please refer to Figure 4 Taking the second etching step alone as an example, when the process parameters of the pre-etching step and the main etching step adopt the process parameters shown in Table 1, a Fig. 6A The first sub-groove 1111 and Figure 6CThe second sub-groove 1112 is shown. The etching depth hc of the first sub-groove 1111 is about 1.48 μm, and the etching depth hd of the second sub-groove 1112 is about 2 microns. The etching depth hc of the first sub-groove 1111 is significantly smaller than the etching depth hd of the second sub-groove 1112. This indicates that in the second etching step, the etching rate of the first portion of the substrate 11 is smaller than the etching rate of the second portion of the substrate 11. Figure 6B It can be seen that microgrooves 1111B are formed at the corners of the first subgrooves 1111, which indicates that the microgroove effect can be generated in the second etching step. Furthermore, when the film layer 10 to be etched is disposed on the wafer, the difference between the etching depth hd of the second subgrooves 1112 located in the center area of the wafer and the etching depth hd of the second subgrooves 1112 located in the edge area of the wafer is about 0.009 μm, which also proves that etching the substrate 11 using the second etching step also has good etching uniformity.
[0075] Table 2 Process parameters of each step of the second etching step in the second example
[0076]
[0077] Please refer to Figure 4 Continuing to take the second etching step alone as an example, when the process parameters in the pre-etching step and the main etching step adopt the process parameters shown in Table 2, a Fig. 7A The first sub-groove 1111 and Figure 7B The second sub-groove 1112 shown in the figure, wherein a micro-groove 1111B is also formed at the bottom of the first sub-groove 1111. In the second example, the upper electrode center power of the main etching step is 350W×55%=192.5W, and the upper electrode center power of the main etching step in the first example is 600W×80%=480W. The upper electrode center power of the main etching step in the second example is smaller than that of the main etching step in the first example, so that the micro-groove effect of the second example is not as obvious as the micro-groove effect of the first example. The etching depth hc of the first sub-groove 1111 is about 0.97μm, and the etching depth hd of the second sub-groove 1112 is about 1 micron. The etching depth difference between the first sub-groove 1111 and the second sub-groove 1112 is about 3% of the etching depth hd of the second sub-groove 1112, which can also prove that the etching of the substrate 11 using the second etching step has good uniformity.
[0078] In addition, in the first example and the second example, the sidewall of the first sub-groove 1111 is slightly inclined, with an angle of about 85° to 87° (including the end points), and the sidewall of the second sub-groove 1112 is vertical.
[0079] Other process conditions of the second etching step also include: the temperature range of the wafer carrier is -10℃~100℃ (including endpoint values), which is preferably 0℃; the duty cycle range of the lower electrode power is 10%~90% (including endpoint values); the distribution ratio range of the upper electrode edge power is 10%~90% (including endpoint values); the chamber pressure range is 2mTorr~200mTorr (including endpoint values), the lower electrode power range is 10W~1000W (including endpoint values), and the flow rate range of various gases is 5sccm~500sccm (including endpoint values); the process time is determined according to the etching rate and etching depth of the substrate 11.
[0080] In one embodiment, Figure 5 As shown, the first etching step is an etching step for producing a bottom fillet, and the first etching step includes a sub-cycle of cyclically executing a deposition step, a physical bombardment step, and a chemical etching step; wherein, in each sub-cycle, the deposition step, the physical bombardment step, and the chemical etching step are executed in sequence. For example, step S110 may include: step S111, first executing the deposition step; step S112, then executing the physical bombardment step; step S113, finally executing the chemical etching step.
[0081] In all wheel cycles, the method further comprises at least one of the following:
[0082] The deposition time of the deposition step increases in sequence according to the number of cycles of the sub-cycle;
[0083] The power of the lower electrode in the physical bombardment step increases in sequence according to the number of cycles of the sub-cycle;
[0084] The etching time of the chemical etching step decreases in sequence according to the number of sub-cycles.
[0085] In the related art, since the dry etching process is accompanied by physical bombardment and chemical etching, the bottom morphology of the process will be arc-shaped due to the isotropy of chemical etching, that is, a bottom rounded corner will appear. FIG. 3A to FIG. 3DBy configuring the sub-cycles of the deposition step, the physical bombardment step and the chemical etching step in the first etching step, the Bosch process of the prior art can be optimized, so that the deposition step, the physical bombardment step and the chemical etching step are alternately cycled for multiple rounds, which can gradually increase the lower electrode power of the physical bombardment step as the etching depth increases, allowing more plasma to enter the bottom of the groove to maintain the verticality of the side wall of the first groove 111, and / or gradually extend the deposition time of the deposition step to maintain the verticality of the side wall of the first groove 111, and / or gradually shorten the etching time of the chemical etching step to reduce the effect of isotropic etching on the first groove 111, so as to maintain the verticality of the side wall of the first groove 111. Based on this, the bottom fillet 1111A of the first groove 111 can be reduced.
[0086] For example, Figure 5 As shown, in two adjacent cycles, the increase in the deposition time of the deposition step can be a first preset value, the increase in the upper electrode power can be a second preset value, and the decrease in the etching time of the chemical etching step can be a third preset value. The first preset value Δt1 can be based on the preset initial deposition time t1 init , target deposition time t1 final , the total number of sub-cycles N total And the total number of rounds of the total cycle M total The calculation relationship is shown in the following formula (1):
[0087]
[0088] The second preset value can be based on the preset initial lower electrode power P init , target lower electrode power P final , the total number of sub-cycles N total And the total number of rounds of the total cycle M total The calculation relationship is shown in the following formula (2):
[0089]
[0090] The third preset value Δt2 can be based on the preset initial etching time t2 init , target etching time t2 final , the total number of sub-cycles N total And the total number of rounds of the total cycle M total The calculation relationship is shown in the following formula (3):
[0091]
[0092] Among them, the initial deposition time t1 init , target deposition time t1final , initial lower electrode power P init , target lower electrode power P final , initial etching time t2 init , target etching time t2 final , the total number of sub-cycles N total And the total number of rounds of the total cycle M total Can be preset during the initialization step.
[0093] In the nth round cycle, the deposition time, the lower electrode power and the etching time can be respectively:
[0094]
[0095] Wherein, n is an integer greater than or equal to 0. In addition, Figure 5 In the formula, m represents the number of cycles in the total cycle, and m is also an integer greater than or equal to 0.
[0096] In one example, the initial deposition time t1 init , target deposition time t1 final , initial lower electrode power P init , target lower electrode power P final , initial etching time t2 init , target etching time t2 final , the total number of sub-cycles N total And the total number of rounds of the total cycle M total They can all be preset as constant values, so that the first preset value Δt1, the second preset value ΔP and the third preset value Δt2 are all constant values. In this way, in all wheel cycles, the deposition time of the deposition step can be gradually increased by the same increment, the lower electrode power of the physical bombardment step can be gradually increased by the same increment, and the etching time of the chemical etching step can be gradually decreased by the same decrement, which is beneficial to maintain the verticality of the sidewall of the first groove 111, so as to reduce or eliminate the bottom fillet of the first groove 111.
[0097] In another example, in all rounds of the total cycle, the method of forming the groove further includes at least one of the following:
[0098] The increment of the deposition time increases in sequence according to the number of cycles of the total cycle;
[0099] The increment of the lower electrode power in the physical bombardment step increases in sequence according to the number of cycles of the total cycle;
[0100] The increment of etching time of the chemical etching step decreases in sequence according to the number of cycles of the total cycle.
[0101] For example, the initial deposition time t1 can be preset in the initialization step. init , target deposition time t1final , initial lower electrode power P init , target lower electrode power P final , initial etching time t2 init , target etching time t2 final And the total number of rounds of the total cycle M total are all constant values, and the initial etching time t2 init and target etching time t2 final equal, and the total number of sub-cycles N is preset total According to the total number of cycles M total The first preset value Δt1, the second preset value ΔP and the third preset value Δt2 of each round cycle in the same total cycle are fixed values, and the first preset value Δt1 and the second preset value ΔP are also fixed according to the number of cycles M of the total cycle. total Among them, the initial deposition time t1 init Can be equal to 3.5s, target deposition time t1 final It can be equal to 6s. Initial lower electrode power P init It can be equal to 100W, the target lower electrode power P final It can be equal to 120W. Initial etching time t2 init and target etching time t2 final In this way, in all rounds of total cycles, the deposition time of the deposition step can be gradually increased by a gradually increasing amount, and the lower electrode power of the physical bombardment step can be gradually increased by a gradually increasing amount, which is also conducive to maintaining the verticality of the sidewall of the first groove 111 to reduce or eliminate the bottom rounded corner of the first groove 111.
[0102] For example, in the initialization step, the initial deposition time t1 may be preset. init , target deposition time t1 final , initial lower electrode power P init , target lower electrode power P final , initial etching time t2 init , target etching time t2 final And the total number of rounds of the total cycle M total are all constant values, and the initial deposition time t1 init Equal to the target deposition time t1 final , initial lower electrode power P init Equal to the target lower electrode power P final , and the total number of sub-cycles N is preset total According to the total number of cycles M totalIncreasing successively, the first preset value Δt1, the second preset value ΔP and the third preset value Δt2 of each round cycle in the same total cycle can be fixed values, and the third preset value Δt2 is based on the total number of cycles M. total Decrease in sequence. Among them, the initial etching time t2 init It can be equal to 3.6s, and the target etching time can be equal to 0.6s. It should be noted that the various parameters in this example can be selected and adjusted according to actual needs, and the embodiments of the present application are not limited to this. In this way, in all total cycles, the etching time of the chemical etching step can be gradually reduced by a gradually decreasing amount, which is also conducive to maintaining the verticality of the sidewalls of the first groove 111 to reduce or eliminate the bottom fillet of the first groove 111.
[0103] In one embodiment, the first groove 111 is used as a cavity of a MEMS structure or as a chip accommodating cavity of a buried fan-out packaging structure. In other words, the method for forming a groove in an embodiment of the present application can be used to form a cavity of a MEMS structure or to form a chip accommodating cavity of a buried fan-out packaging structure. The following describes an embodiment of forming a cavity of a MEMS structure and a chip accommodating cavity of a buried fan-out packaging structure using the method for forming a groove in the present application.
[0104] For example, please refer to FIG. 8A to FIG. 8D As shown, the method for forming a groove can be used to form a cavity of a MEMS structure, and the method can include the following steps S310 to S340.
[0105] Step S310: Fig. 8A As shown, a film layer 10 to be etched is provided; the film layer 10 to be etched includes a stacked substrate 11, a mask layer 12, and a first passivation layer 13, an accessory layer 14, and a second passivation layer 15 located on a surface of the substrate 11 facing away from the mask layer 12 and stacked. The mask layer 12 is provided with a first mask opening 12A and a second mask opening 12B, and the opening size of the first mask opening 12A is larger than the opening size of the second mask opening 12B.
[0106] Step S320: Figure 8B As shown, the first etching step and the second etching step of the embodiment of the present application are performed alternately and cyclically, and the first portion of the substrate 11 exposed from the first mask opening 12A and the second portion exposed from the second mask opening 12B are simultaneously etched until the first passivation layer 13 is exposed, so as to simultaneously form the first groove 111 and the second groove 112 in the substrate 11; the opening size of the first groove 111 is larger than the opening size of the second groove 112, and the etching depth of the first groove 111 is less than or equal to the etching depth of the second groove 112.
[0107] Step S330: Figure 8CAs shown, the first passivation layer 13 is etched from the area exposed by the first mask opening 12A and the second mask opening 12B until the accessory layer 14 is exposed. The accessory layer 14 includes a diaphragm layer 141 and a back plate layer 142 that are stacked and spaced apart. The diaphragm layer 141 is provided with a first through hole 1411, and a first pad 1412 is provided on the surface of the diaphragm layer 141 facing away from the substrate 11. The back plate layer 142 is provided with a plurality of second through holes 1421, and a second pad 1422 is provided on the surface of the back plate layer 142 facing away from the substrate 11. The orthographic projection of the first through hole 1411 on the substrate 11 overlaps with the orthographic projection of a second through hole 1421 on the substrate 11. The first through hole 1411, the second through hole 1421, and the space between the diaphragm layer 141 and the back plate layer 142 are all filled with passivation material.
[0108] Step S340: Fig.8D As shown, the second passivation layer 15 is removed and the passivation materials in the first through hole 1411, in the second through hole 1421 and between the first through hole 1411 and the second through hole 1421 are removed, so that the first groove 111 and the first through hole 1411 are interconnected, the first through hole 1411 and the plurality of second through holes 1421 are interconnected, and the first groove 111 constitutes a cavity of the microphone.
[0109] In this embodiment, by alternately executing the first etching step and the second etching step in a cycle, not only can the bottom fillet of the first groove 111 be eliminated, so that the bottom of the cavity of the microphone formed by the first groove 111 is flat; but also the first groove 111 and the second groove 112 with different opening sizes can be formed at the same time, and the etching depth of the second groove 112 with a small opening size is equal to or greater than the etching depth of the first groove 111 with a large opening size, which is beneficial to simplifying the process steps and reducing the process cost.
[0110] It should be noted that in the process of forming the cavity of the MEMS structure using the method of the embodiment of the present application, the method of forming each membrane layer of the MEMS structure and the selected process parameters can refer to conventional technical means in the field and will not be described in detail here.
[0111] Exemplarily, the method for forming a groove may also be used to form a chip accommodating cavity of a buried fan-out packaging structure, and the method includes the following steps S410 to S470.
[0112] Step S410: Fig. 9A As shown, a film layer 10 to be etched is provided, and the film layer 10 to be etched includes a stacked substrate 11 and a mask layer 12, and the mask layer 12 is provided with a first mask opening 12A and a second mask opening 12B, and the opening size of the first mask opening 12A is larger than the opening size of the second mask opening 12B.
[0113] Step S420: Fig. 9B As shown, the first etching step and the second etching step are performed alternately, the first portion of the substrate 11 exposed from the first mask opening 12A is etched to a first target depth h1 to form a first groove 111 in the substrate 11, and the second portion of the substrate 11 exposed from the second mask opening 12B is etched to a second target depth h2 to simultaneously form a second groove 112 in the substrate 11; the first target depth h1 is less than the second target depth h2.
[0114] Step S430: Fig. 9C As shown, after removing the mask layer 12 , the first chip 31 is placed in the first trench 111 , so that the first trench 111 is used as a chip accommodating cavity for the first chip 31 .
[0115] Step S440: Fig.9D As shown, a metal connection structure 113 is arranged in the second groove 112 and a redistribution line 114 is arranged on the side surface of the substrate 11 where the first chip 31 is placed, so that the first chip 31 is connected to the redistribution line 114, and the redistribution line 114 is connected to the metal connection structure 113.
[0116] Step S450: Fig.9E As shown, a temporary bonding plate 115 is arranged on the side of the substrate 11 where the first chip 31 is placed, and the surface of the substrate 11 facing away from the first chip 31 is thinned so that the second groove 112 forms a through hole penetrating the substrate 11 and exposes one end of the metal connection structure 113 away from the first chip 31.
[0117] Step S460: Fig.9F As shown, a metal ball 116 is disposed on the surface of the side of the substrate 11 away from the first chip 31, and after the metal ball 116 is attached to the end of the metal connection structure 113 away from the first chip 31, the second chip 32 is pressed and fixed on the metal ball 116, so that the second chip 32 is stacked with the first chip 31. In step S460, a redistribution line can also be disposed on the surface of the side of the substrate 11 away from the first chip 31, so as to connect the second chip 32 and the end of the metal connection structure 113 away from the first chip 31 by using the redistribution line, so as to ensure that the first chip 31 and the second chip 32 located on opposite sides of the substrate 11 can be connected to each other through the metal connection structure 113 in the through hole.
[0118] Step S470: Figure 9G As shown, the temporary bonding plate 115 is removed, and a metal ball 116 is arranged at one end of the pins of the first chip 31 and the metal connection structure 113 close to the first chip 31, thereby finally forming an embedded fan-out packaging structure.
[0119] In this embodiment, by alternately performing the first etching step and the second etching step, not only can the bottom fillet of the first groove 111 be eliminated, so that the bottom of the chip cavity formed by the first groove 111 is flat, which has an adverse effect on the placement of the first chip 31; but also the first groove 111 and the second groove 112 with different opening sizes can be formed at the same time, and the etching depth of the second groove 112 with a small opening size is equal to or greater than the etching depth of the first groove 111 with a large opening size, without the need to form the first groove 111 and the second groove 112 separately, which is conducive to simplifying the process steps and reducing the process cost. Moreover, after the metal connection structure 113 is provided in the second groove 112, when the side surface of the substrate 11 facing away from the first chip 31 is thinned, it can be ensured that the second groove 112 forms a through hole and leaks out the end of the metal connection structure 113 without damaging the chip cavity.
[0120] It should be noted that in the process of forming the chip accommodating cavity of the buried fan-out packaging structure using the method of the embodiment of the present application, the method of forming each film layer of the buried fan-out packaging structure and the selected process parameters can refer to the conventional technical means in the field and will not be described in detail here.
[0121] An embodiment of the present application also provides a semiconductor process equipment, including a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, the controller including at least one processor and at least one memory, the memory storing a computer program, and when the computer program is executed by the processor, a method of any of the above-mentioned embodiments is implemented.
[0122] Fig.10 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application.
[0123] like Fig.10 As shown, the semiconductor process equipment 200 may include a process chamber 20, an inlet assembly 20A, an upper electrode assembly 20B and a lower electrode assembly 20C, a gas extraction assembly 20D and a controller ( Fig.10 The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method of any one of the above embodiments is implemented.
[0124] Exemplarily, the controller can be a host computer or a slave computer. The controller can control the valve opening of the air inlet component 20A to introduce the corresponding process gas into the process chamber 20; the controller can also control the opening and closing degree of the valve of the air inlet component 20A to control the flow rate of the process gas. The controller can also control the exhaust component 20D to exhaust the interior of the process chamber 20, such as controlling the valve opening degree or the exhaust pump speed of the exhaust component 20D, to control the pressure inside the process chamber 20, discharge reaction byproducts, etc.
[0125] The upper electrode assembly 20B may include an RF coil 21, an upper RF power source 23 and an upper matcher 25. The controller is also used to control the upper RF power source 23 to provide RF power to the RF coil 21 through the upper matcher 25, so that the RF coil 21 excites the process gas inside the process chamber 20 to generate plasma A.
[0126] The lower electrode assembly 20C may include a wafer carrier 22, a lower RF power supply 24, and a lower matcher 26. The controller is also used to control the lower RF power supply 24 to provide RF power to the wafer carrier 22 through the lower matcher 26 to provide RF bias. The wafer carrier 22 may be, for example, an electrostatic chuck, a mechanical chuck, or a vacuum adsorption chuck. The wafer carrier 22 is used to carry a wafer provided with a film layer 10 to be etched according to an embodiment of the present application.
[0127] The semiconductor process equipment 200 of the embodiment of the present application may be an inductively coupled plasma (ICP) device or a capacitively coupled plasma (CCP) device. The embodiment of the present application does not limit the type of the semiconductor process equipment 200.
[0128] In this application, unless otherwise clearly specified and limited, the terms "connected", "connected", "stacked" and the like should be understood in a broad sense. For example, they can be fixedly connected, detachably connected, or integrated; they can be directly connected, or indirectly connected through an intermediate medium, and they can be internally connected between two elements or an interactive relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to the specific circumstances. The terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one such feature. In the description of this application, "multiple" means two or more, unless otherwise clearly and specifically limited.
[0129] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they contradict each other.
[0130] It should be understood that the various parts of the present application can be implemented with hardware, software, firmware or a combination thereof. In the above embodiments, multiple steps or methods can be implemented with software or firmware stored in a memory and executed by a suitable instruction execution system. All or part of the steps of the above embodiment method can be completed by instructing the relevant hardware through a program, which can be stored in a computer-readable storage medium, and when the program is executed, it includes one of the steps of the method embodiment or a combination thereof.
[0131] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for forming a groove, characterized in that: Applied to a film layer to be etched, the film layer to be etched comprises a stacked substrate and a mask layer, the mask layer is provided with a first mask opening, and the method comprises: Alternating and cyclically performing a first etching step and a second etching step to form a first trench in the substrate; Wherein, in each total cycle, the first etching step is used to etch the first portion of the substrate exposed from the first mask opening to a first predetermined depth, and the second etching step is used to etch the first portion of the substrate exposed from the first mask opening to a second predetermined depth; Furthermore, in each total cycle, one of the first etching step and the second etching step generates a bottom rounded corner, and the other of the first etching step and the second etching step generates a micro-groove effect.
2. The method according to claim 1, characterized in that The mask layer is further provided with a second mask opening, the second mask opening exposes a second portion of the substrate, and the opening size of the second mask opening is smaller than the opening size of the first mask opening; The method further comprises: In the process of performing the first etching step and the second etching step alternately and cyclically, a second trench is also formed in the substrate; In each total cycle, in the etching step of producing bottom fillet, the etching rate of the first part is greater than the etching rate of the second part, and in the etching step of producing micro-groove effect, the etching rate of the first part is less than the etching rate of the second part.
3. The method according to claim 2, characterized in that In each total cycle, the second portion is etched to a third predetermined depth, and the third predetermined depth is equal to or greater than the sum of the first predetermined depth and the second predetermined depth.
4. The method according to claim 1 or 2, characterized in that: The second etching step is an etching step for generating a micro-groove effect. The second etching step includes a main etching step. The process conditions of the main etching step include: the range of the upper electrode center power and the upper electrode edge power are both 100W to 500W.
5. The method according to claim 4, characterized in that At least one of the upper electrode center power and the upper electrode edge power is less than 200W.
6. The method according to claim 4, characterized in that The second etching step further includes a pre-etching step, which is performed before the main etching step; the pre-etching step is used to remove etching by-products formed in the first etching step.
7. The method according to claim 6, characterized in that The material of the substrate is a silicon-containing material, the process conditions of the pre-etching step include that the etching gas includes a carbon-containing and fluorine-containing gas, and the process conditions of the main etching step include that the etching gas includes a sulfur-containing and fluorine-containing gas and oxygen.
8. The method according to claim 1 or 2, characterized in that: The first etching step is an etching step for generating a bottom fillet, and the first etching step includes a sub-cycle of cyclically executing a deposition step, a physical bombardment step, and a chemical etching step; wherein, in each round of the sub-cycle, the deposition step, the physical bombardment step, and the chemical etching step are sequentially executed; in all rounds of the sub-cycle, the method further includes at least one of the following: The deposition time of the deposition step increases in sequence according to the number of cycles of the sub-cycle; The power of the lower electrode in the physical bombardment step is increased in sequence according to the number of cycles of the sub-cycle; The etching time of the chemical etching step decreases in sequence according to the number of cycles of the sub-cycles.
9. The method according to claim 8, characterized in that In all rounds of the total cycle, the method further includes at least one of the following: The increment of the deposition time increases in sequence according to the number of cycles of the total cycle; The increment of the power of the lower electrode in the physical bombardment step increases in sequence according to the number of cycles of the total cycle; The increment of the etching time of the chemical etching step decreases in sequence according to the number of cycles of the total cycle.
10. The method according to claim 8, characterized in that In the nth round cycle, at least one of the deposition time t1, the lower electrode power P and the etching time t2 satisfies the following relationship: Among them, t1 init is the initial deposition time, t1 final is the target deposition time, N total is the total number of sub-cycles, M total is the total number of rounds in the total cycle, P init is the initial lower electrode power, P final is the target lower electrode power, t2 init is the initial etching time, t2 final is the target etching time, n, N total and M total All are positive integers.
11. The method according to claim 1, characterized in that: The first groove is used as a cavity of a MEMS structure or as a chip accommodating cavity of an embedded fan-out packaging structure.
12. A semiconductor process equipment, comprising a process chamber, an air inlet assembly, an upper electrode assembly, a lower electrode assembly and a controller, characterized in that: The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method according to any one of claims 1 to 11 is implemented.