Negative electrode material and preparation method and application thereof

By using a small-sized core to deposit nano-silicon and mixed carbon source slurry in the silicon-carbon negative electrode material to form a "rebar-cement" structure, the problem of long lithium ion transmission paths and many material interfaces in lithium-ion batteries is solved, and the rate is increased. and cycle performance, reducing side reactions and improving electrochemical performance.

CN118771385AActive Publication Date: 2024-10-15HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202410891509.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-15
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing silicon-carbon anode materials in lithium-ion batteries have poor rate performance and poor cycle performance due to long lithium ion transmission paths, multiple material interfaces, and large specific surface areas. They are also prone to side reactions with electrolytes, affecting the long cycle life of the battery. performance.

Method used

A small-sized core is used to deposit nano-silica, and the core is granulated and surface modified by mixing carbon source slurry to form a "rebar-cement" structure. Single-arm carbon tubes are used to penetrate and connect the core pores to shorten the particle size of lithium ion transmission. , reduce the specific surface area and improve ion and electron transport efficiency.

Benefits of technology

It significantly improves the rate performance and cycle performance of the silicon-carbon anode material, enhances the structural strength and expansion resistance, reduces side reactions with the electrolyte, and improves the electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771385A_ABST
    Figure CN118771385A_ABST
Patent Text Reader

Abstract

The invention discloses a negative electrode material as well as a preparation method and application thereof, and belongs to the technical field of lithium ion batteries. A single particle of the silicon-carbon negative electrode material comprises one or more inner cores of 1-4 microns, each inner core is of a porous structure, a conductive single-arm carbon tube transversely penetrating through a pore channel exists in each inner core, a conductive carbon layer exists outside each inner core, and carbon tubes and graphene are dispersed and distributed in the carbon layers to form a conductive 3D network. According to the invention, nano silicon is deposited on small-size cores, the lithium ion transmission particle size is shortened, then granulation and surface modification are carried out on the cores through the mixed carbon source slurry, one or more cores are compounded to form a finished product with a slightly large size, and through the core composite single-arm carbon tube, each pore channel of the cores is connected in a penetrating manner, so that the lithium ion battery is obtained. An ion and electron transport fast channel is improved, and the rate capability of the material is improved; the formed reinforcing steel bar-cement type structure enhances the structural strength of the inner core, enhances the expansion resistance of the material, and enhances the electrochemical performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a negative electrode material and a preparation method and application thereof. Background Art

[0002] At present, the application scenarios of lithium-ion batteries are gradually increasing, and high energy density and long cycle requirements are put forward for lithium-ion batteries. There are usually the following methods to improve energy density: (1) increase the gram capacity of the positive electrode material, but the gram capacity of the positive electrode material has been developed to the limit; (2) reduce the electrolyte retention coefficient, but it will affect the cycle; (3) reduce the weight of the shell; (4) increase the gram capacity of the negative electrode. The high gram capacity of the silicon negative electrode has attracted much attention, but during the charging and discharging process of silicon, the lithium insertion and extraction reaction of silicon will be accompanied by a large volume change (>300%), causing the destruction of the material structure and mechanical pulverization, resulting in the separation of electrode materials and electrode materials and current collectors, separation between particles, and then loss of electrical contact, resulting in rapid capacity decay and deterioration of cycle performance. Due to the drastic volume effect, the SEI film on the silicon surface is in a dynamic process of destruction-reconstruction, and has many side reactions with the battery cell, which will cause continuous lithium ion consumption and further affect the cycle performance. At present, the silicon negative electrode industry has two parallel routes: pre-lithium silicon oxygen and new silicon carbon. Although pre-lithium silicon oxygen is relatively mature and has good batch stability, new silicon carbon has become a hot spot for the research and development of silicon negative electrodes due to its low expansion and good cycle. At present, the new silicon carbon is mainly prepared by depositing nanosilicon in the pores of porous carbon matrix. The microporous structure of porous carbon matrix will inhibit the growth of silicon. Therefore, all prepared are amorphous / microcrystalline nanosilicon, which has excellent cycle performance. However, this type of new silicon carbon material has a multi-porous structure, and the lithium ion transmission path inside the material is long, and there are many silicon-carbon interfaces in the material, which affects the lithium ion deintercalation; therefore, the rate performance of this material is poor. In addition, this material is mostly a microporous carbon matrix with a large specific surface area, which is difficult to coat completely and evenly, resulting in a large specific surface area of ​​the material and more side reactions with the electrolyte. Summary of the invention

[0003] The purpose of the present invention is to provide a negative electrode material and a preparation method and application thereof. The silicon-carbon negative electrode material of the present invention has the characteristics of high rate performance and long cycle performance.

[0004] The present invention first provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps: (1) dispersing the single-arm carbon nanotubes in a solvent to obtain a solution A; and then mixing the solution A with a formaldehyde solution to obtain a solution B; (2) dissolving bisphenol A in the solution B, heating it, and then adding a catalyst to adjust the pH of the solution to 7-10, so that the solution is completely solidified to obtain a solid C; crushing the solid C to obtain a carbon precursor D; (3) mixing the carbon precursor D and the alkaline activator, calcining, and obtaining a mixture E; washing the mixture E, and obtaining a porous carbon matrix F; (4) placing the porous carbon substrate F into a fluidized bed, introducing a mixed gas of silane and nitrogen, and heating and keeping the temperature; then introducing a mixed gas of acetylene and argon, and heating and keeping the temperature, to obtain product G; (5) Depositing carbon on the surface of product G by chemical vapor deposition to obtain product H; (6) The product H is mixed with a mixed carbon source slurry, and calcined to obtain the silicon-carbon negative electrode material.

[0005] The method of the present invention uses a small-sized core to deposit nano-silicon, shortening the lithium ion transmission particle size, and then granulates and surface-modifies the core by mixing a carbon source slurry, composites one or more cores to form a finished product with a slightly larger size, and composites single-arm carbon tubes through the core to connect various channels of the core, thereby improving the rapid channel for ion and electron transport and improving the material rate performance; the graphene and carbon tubes in the mixed carbon source slurry form a "rebar-cement" structure in the outer coating layer, thereby increasing the structural strength of the core, increasing the material's anti-expansion property, and improving its electrochemical performance.

[0006] In the above-mentioned method for preparing the silicon-carbon negative electrode material, in step (1), the diameter of the single-arm carbon tube is 0.5-1 nm, and the length of the tube is 2-20 nm; The solvent is anhydrous ethanol; In the solution A, the solid content of the single-arm carbon tube is 0.5% to 5%; The mass percentage concentration of the formaldehyde solution is 35-37%; The mass ratio of the single-arm carbon tube to formaldehyde is 1:35-80; In step (2), the mass ratio of bisphenol A to solution B is 1:5-8; The catalyst is at least one of sodium carbonate solution, sodium hydroxide solution and ammonium hydroxide solution; specifically, the concentration of the sodium carbonate solution, sodium hydroxide solution or ammonium hydroxide solution is 0.5-1 mol / L; more specifically, it can be 0.5 mol / L; The solid C is crushed into block particles with a particle size of 1-4 μm, which is the carbon precursor D.

[0007] In the above-mentioned method for preparing the silicon-carbon negative electrode material, in step (2), the heating temperature is 180-200°C.

[0008] The specific operation of step (2) of the above-mentioned method for preparing the silicon-carbon negative electrode material is as follows: dissolving bisphenol A in the solution B, heating the resulting solution to 180-200° C., then dropping a catalyst to adjust the solution pH to 7-10, stopping when solid begins to appear in the solution, and continuing stirring until the solution is completely solidified to obtain solid C; crushing the solid C to obtain a carbon precursor D.

[0009] In the above-mentioned method for preparing the silicon-carbon negative electrode material, in step (3), the alkaline activator is at least one of potassium hydroxide, sodium hydroxide and lithium hydroxide; The mass ratio of the carbon precursor D to the alkaline activator is 1:1-4; The calcination is carried out in an inert atmosphere; specifically, the inert atmosphere is a nitrogen or argon atmosphere; The calcination temperature is 700-900°C; the calcination time is 1-5h; The washing is carried out in sequence with a hydrochloric acid solution and water; specifically, the concentration of the hydrochloric acid is 0.1-2 mol / L, and specifically can be 0.2 mol / L.

[0010] In the above-mentioned method for preparing the silicon-carbon negative electrode material, in step (3), the washing operation is as follows: placing the mixture E in a hydrochloric acid solution and stirring and washing for 10 to 60 minutes, and then washing with water for multiple times until the solution pH is ≤8; Specifically, the mass ratio of the mixture E to the hydrochloric acid solution may be 1:2-5.

[0011] The pore size of the porous carbon matrix F is 0.3-3 nm, and the specific surface is 1600-2200 nm. 2 / g, and the pore volume is 0.8~1.0 cc / g.

[0012] The specific operation of step (4) of the above-mentioned method for preparing silicon-carbon negative electrode material is as follows: the porous carbon substrate F is placed in a fluidized bed, a silane and nitrogen mixture with a volume ratio of 5:1 to 1:5 is introduced, and the temperature is kept at 400 to 700° C. for 2 to 6 hours; then, a acetylene and argon mixture with a gas flow ratio of 2:1 to 1:3 is introduced, and the temperature is kept at 650 to 750° C. for 1 to 3 hours to obtain product G; The silane is one of monosilane or disilane.

[0013] The specific operation of step (5) of the above-mentioned method for preparing the silicon-carbon negative electrode material is as follows: placing the product G in a chemical vapor deposition reactor, introducing a mixture of acetylene and argon at a gas flow ratio of 2:1 to 1:2, and maintaining the temperature at 650 to 750° C. for 1 to 4 hours to obtain the product H.

[0014] In the above-mentioned method for preparing the silicon-carbon negative electrode material, in step (6), the mass ratio of the product H to the mixed carbon source slurry is 10:1 to 15:1; The mixed carbon source slurry is obtained by dispersing graphene, carbon tubes and low-temperature asphalt in anhydrous ethanol; specifically, the mass ratio of the graphene, carbon tubes and low-temperature asphalt can be 1:1:2; the solid content of the mixed carbon source slurry can be 30% to 40%; the diameter of the carbon tube can be a single-arm carbon tube of 3 to 20 nm; The calcination is carried out in an inert atmosphere; specifically, the inert atmosphere is a nitrogen or argon atmosphere; The calcination temperature is 600-900° C. and the calcination time is 4-6 hours.

[0015] The low-temperature asphalt is asphalt with a softening point below 200°C; specifically, it can be at least one of Xinjiang Zhongtan 150# coated asphalt and 180# coated asphalt; The present invention further provides a silicon-carbon negative electrode material prepared by the above preparation method.

[0016] Specifically, the particle size of the silicon-carbon negative electrode material is 3-10 μm.

[0017] The application of the above-mentioned silicon-carbon negative electrode material in the preparation of lithium-ion battery negative electrode also falls within the protection scope of the present invention.

[0018] The silicon-carbon negative electrode material of the present invention comprises a single particle containing one or more inner cores of 1 to 4 μm, wherein the inner core is one or more porous carbon matrices with a porous structure, wherein nano-silicon particles are confinedly grown in the pores thereof, and conductive single-arm carbon tubes are present inside the inner core and cross the pores, and a conductive carbon layer is present outside the inner core, wherein carbon tubes and graphene are dispersedly distributed in the carbon layer to form a conductive 3D network.

[0019] The present invention has the following beneficial effects: (1) The silicon-carbon negative electrode material of the present invention uses a small-sized core (1-3 μm porous carbon matrix) to deposit nano-silicon, shortening the lithium ion transmission particle size; then the core is granulated and surface-modified by using a mixed carbon source slurry; the core is coated with asphalt in the mixed carbon source slurry or multiple cores are wrapped by granulation, and a high ion conductor carbon layer is formed on the surface of the core after carbonization, which can also reduce the specific surface area of ​​the material (the particle size becomes larger), reduce the negative reaction with the electrolyte, and improve the first effect (SEI film is reduced); (2) The graphene and carbon tubes in the mixed carbon source slurry form a conductive network between the cores in a single fast-charging long-cycle silicon-carbon material particle, increasing the connection strength of each core and forming a "rebar-cement" structure. The entire outer coating layer and the inner core porous carbon matrix inhibit the expansion of silicon and improve the electrochemical performance of the material. (3) Single-arm carbon nanotubes are compounded into the carbon precursor. The porous carbon matrix, i.e., the inner core, contains single-arm carbon nanotubes that penetrate and connect the various pores of the inner core, thereby improving the rapid channels for ion and electron transport and the rate performance of the material. In addition, the inner core itself also forms a "rebar-cement" structure, which increases the structural strength of the inner core (porous carbon matrix), increases the material's anti-expansion property, and improves its electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XRD diagram of the fast-charging and long-cycle silicon-carbon negative electrode material prepared in Example 2 of the present invention.

[0021] Figure 2 Schematic diagram of the structure of the porous carbon matrix F of the present invention.

[0022] Figure 3 This is a schematic diagram of the structure of the fast-charging and long-cycle silicon-carbon negative electrode material of the present invention.

[0023] Figure 4 This is a graph showing the cycling results of a 7Ah soft-pack battery using the fast-charging, long-cycle silicon-carbon negative electrode material prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.

[0025] The experimental methods in the following examples are all conventional methods unless otherwise specified.

[0026] The quantitative tests in the following examples were all repeated three times, and the results were averaged.

[0027] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0028] Low temperature asphalt is one of Xinjiang Zhongtan 150# coated asphalt or 180# coated asphalt; Example 1 (1) Dispersing single-arm carbon nanotubes with a diameter of 0.5 nm and a length of 2 nm in anhydrous ethanol to form a solution with a solid content of 0.5% (mass fraction), and then adding a 36% formaldehyde solution with a mass ratio of single-arm carbon nanotubes to formaldehyde of 1:35 to obtain solution B; (2) Bisphenol A was heated to 170°C, then added to solution B and stirred. The mass ratio of bisphenol A to solution B was 1:5. The resulting solution was heated to 180°C, and 0.5 mol / L sodium carbonate solution was added dropwise to adjust the pH of the solution to 7. The solution was stopped when solid began to appear, and stirring was continued until it was completely solidified to obtain solid C. Solid C was then crushed into block particles with a particle size of 1 μm to obtain carbon precursor D. (3) The carbon precursor D and potassium hydroxide were mixed evenly in a mass ratio of 1:1, and calcined at 700 °C for 1 h under a nitrogen atmosphere to obtain a mixture E; then the mixture was placed in a 0.2 mol / L hydrochloric acid solution and stirred for 20 min, wherein the mass ratio of the mixture E to the hydrochloric acid solution was 1:2; after drying, it was washed with distilled water for multiple times until the solution pH was ≤8. After drying, the pore size was 0.3 nm and the specific surface area was 1600 m 2 / g, pore volume of porous carbon matrix F is 0.8cc / g; (4) The porous carbon substrate F was placed in a fluidized bed, and a mixture of monosilane and nitrogen was introduced at a volume ratio of 5:1, heated to 400°C and kept warm for 2 h, and a mixture of acetylene and argon was introduced at a gas flow ratio of 2:1, and kept warm at 650°C for 1 h to obtain product G; (5) Product G was placed in a chemical vapor deposition furnace, and a mixture of acetylene and argon was introduced at a gas flow ratio of 2:1, and the mixture was kept at 650°C for 1 hour to obtain product H; then it was placed in a mixed carbon source slurry, the mass ratio of product H to the mixed carbon source slurry was 10:1, wherein the mixed carbon source slurry was obtained by dispersing graphene, carbon tubes and Xinjiang Zhongtan 150# coated asphalt in anhydrous ethanol at a mass ratio of 1:1:2, and the solid content of the mixed carbon source slurry was 35% (mass fraction), wherein the diameter of the carbon tubes was a single-arm carbon tube with a diameter of 3~20nm; after filtration and drying, it was calcined at 600°C in an argon atmosphere for 4 hours to obtain a finished product I with a particle size of 3μm, i.e., a fast-charging and long-cycle silicon-carbon negative electrode material.

[0029] The obtained fast-charge long-cycle silicon-carbon negative electrode material and metal lithium sheet were assembled into a CR2032 half-cell for electrochemical performance testing. The assembly order was negative electrode shell, metal lithium sheet, diaphragm, fast-charge long-cycle silicon-carbon negative electrode material sheet, gasket, positive electrode shell, and the electrolyte added was Xinzhoubang LBC3021H43. The test was 0.1C (first time) + rate 0.5C (cycle), and the charge and discharge voltage was 0.005~0.8V. The results showed that the discharge specific capacity of the negative electrode sheet can reach 1605 mAh / g, the first efficiency is 81.6%, and after 50 cycles, it can still maintain 81.1% of the capacity.

[0030] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 18:82 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection (Xinzhoubang LBC3021H43) were carried out to assemble 7Ah soft-pack batteries. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The initial efficiency of the battery cell was 86.5%. After 650 cycles of the full battery, the capacity retention rate was 85.5%.

[0031] Example 2 (1) Dispersing single-arm carbon nanotubes with a diameter of 0.8 nm and a length of 5 nm in anhydrous ethanol to form a solution with a solid content of 2% (mass fraction), and then adding a 36% formaldehyde solution with a mass ratio of single-arm carbon nanotubes to formaldehyde of 1:42 to obtain solution B; (2) Bisphenol A was heated to 170°C, then added to solution B and stirred. The mass ratio of bisphenol A to solution B was 1:6. The resulting solution was heated to 190°C, and 0.5 mol / L sodium carbonate solution was added dropwise to adjust the pH of the solution to 8. When solid began to appear in the solution, the solution was stopped and stirred until it was completely solidified to obtain solid C. Solid C was then crushed into block particles with a particle size of 1.5 μm to obtain carbon precursor D. (3) The carbon precursor D and sodium hydroxide were mixed evenly in a mass ratio of 1:2, and calcined at 750 °C for 2 h under a nitrogen atmosphere to obtain a mixture E; then the mixture was placed in a 0.2 mol / L hydrochloric acid solution and stirred for 20 min, wherein the mass ratio of the mixture E to the hydrochloric acid solution was 1:3; after drying, it was washed with distilled water for multiple times until the solution pH was ≤8. After drying, the pore size was 1.2 nm and the specific surface was 1800 m 2 / g, pore volume of porous carbon matrix F is 0.9 cc / g; (4) The porous carbon substrate F was placed in a fluidized bed, and a mixture of monosilane and nitrogen was introduced at a volume ratio of 1:1, heated to 500°C and kept warm for 2 h, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:1.5, and kept warm at 690°C for 2 h to obtain product G; (5) Place product G in a chemical vapor deposition furnace, introduce a mixture of acetylene and argon at a gas flow ratio of 1:1, and keep it at 680°C for 1.5 hours to obtain product H; then put it into a mixed carbon source slurry, the mass ratio of product H to the mixed carbon source slurry is 10:1, wherein the mixed carbon source slurry is graphene, carbon tubes and Xinjiang Zhongtan 180# coated asphalt dispersed in anhydrous ethanol at a mass ratio of 1:1:2, the solid content of the mixed carbon source slurry is 35% (mass fraction), and the diameter of the carbon tube is a single-arm carbon tube with a diameter of 3~20nm; after filtration and drying, calcined at 650°C in an argon atmosphere for 4.5 hours to obtain a finished product I with a particle size of 5μm, that is, a fast-charging and long-cycle silicon-carbon negative electrode material. Figure 1 As shown, the XRD spectrum of the fast-charging and long-cycle silicon-carbon negative electrode material has no obvious silicon characteristic peaks, the internal structure of the material is uniform, and it has good cycle performance.

[0032] The obtained fast-charge and long-cycle silicon-carbon negative electrode material and metal lithium sheet were used to form a CR2032 half-cell for electrochemical performance testing. The assembly order was negative electrode shell, metal lithium sheet, diaphragm, fast-charge and long-cycle silicon-carbon negative electrode material electrode sheet, gasket, and positive electrode shell. The electrolyte added was Xinzhoubang LBC3021H43. The test rate was 0.1C (first time) + 0.5C (cycle). The results showed that the discharge specific capacity of the negative electrode sheet could reach 1680 mAh / g, with an initial efficiency of 82.9%. After 50 cycles, 83.8% of the capacity could still be maintained.

[0033] A 7Ah soft-pack battery was assembled according to the method of Example 1. After the battery was divided into different capacities, a room temperature cycle test was performed at a current density of 1C / 1C. The initial efficiency of the battery cell was 87.5%. After 790 cycles of the full battery, the capacity retention rate was 89.5%.

[0034] Figure 4 This is a full battery cycle result diagram of the fast-charge long-cycle silicon-carbon negative electrode material prepared in Example 2, Figure 4 It can be seen that the full battery has excellent cycle performance. After 790 cycles at room temperature, the capacity retention rate is 89.5%, the trend capacity retention rate is 80%, and the cycle can exceed 1,200 cycles.

[0035] Figure 2 The schematic diagram of the structure of the porous carbon matrix F of the present invention is shown in FIG. The porous carbon matrix F of the present invention is distributed with pores with a pore size of 1.2 nm. The porous carbon matrix F has single-arm carbon tubes penetrating and connecting the pores of the inner core, which improves the fast channel for ion and electron transport and the material rate performance. At the same time, a "rebar-cement" structure is formed, which increases the structural strength of the inner core (porous carbon matrix), increases the material's anti-expansion property, and improves its electrochemical performance.

[0036] Figure 3 The schematic diagram of the structure of the fast-charge long-cycle silicon-carbon negative electrode material of the present invention. The fast-charge long-cycle silicon-carbon negative electrode material of the present invention has multiple small-sized cores (1~3μm porous carbon matrix) deposited with nano-silicon, which shortens the particle size of lithium ion transmission; the core is granulated and surface-modified by mixing carbon source slurry, and a high ion conductor carbon layer is formed on the surface, which can also reduce the specific surface area of ​​the material (the particle size becomes larger), reduce the negative reaction with the electrolyte, and improve the first effect (SEI film reduction). The graphene and carbon tubes in the surface coating layer form a conductive network between the cores in a single fast-charge long-cycle silicon-carbon material particle, increase the connection strength of each core, and form a "reinforced concrete" structure. The entire outer coating layer and the core porous carbon matrix inhibit the expansion of silicon and improve the electrochemical performance of the material.

[0037] Example 3 (1) Dispersing single-arm carbon nanotubes with a diameter of 0.8 nm and a length of 10 nm in anhydrous ethanol to form a solution with a solid content of 2% (mass fraction), and then adding a 36% formaldehyde solution with a mass ratio of single-arm carbon nanotubes to formaldehyde of 1:42 to obtain solution B; (2) Bisphenol A was heated to 170°C, then added to solution B and stirred. The mass ratio of bisphenol A to solution B was 1:6. The resulting solution was heated to 190°C, and 0.5 mol / L sodium carbonate solution was added dropwise to adjust the pH of the solution to 9. The solution was stopped when solid began to appear, and stirring was continued until it was completely solidified to obtain solid C. Solid C was then crushed into block particles with a particle size of 2 μm to obtain carbon precursor D. (3) The carbon precursor D and sodium hydroxide were mixed evenly in a mass ratio of 1:2, and calcined at 750 °C for 2 h under an argon atmosphere to obtain a mixture E; then the mixture was placed in a 0.2 mol / L hydrochloric acid solution and stirred for 20 min, wherein the mass ratio of the mixture E to the hydrochloric acid solution was 1:3; after drying, it was washed with distilled water for multiple times until the solution pH was ≤8. After drying, the pore size was 1.5 nm and the specific surface area was 2050 m 2 / g, and the pore volume is 0.91 cc / g porous carbon matrix F; (4) The porous carbon substrate F was placed in a fluidized bed, and a mixture of monosilane and hydrogen was introduced at a volume ratio of 1:3, heated to 500°C and kept warm for 2 h, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:1.5, and kept warm at 690°C for 2 h to obtain product G; (5) Product G was placed in a chemical vapor deposition furnace, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:1.5, and the mixture was kept at 700°C for 3 hours to obtain product H; then it was placed in a mixed carbon source slurry, and the mass ratio of product H to the mixed carbon source slurry was 10:1, wherein the mixed carbon source slurry was obtained by dispersing graphene, carbon tubes and Xinjiang Zhongtan 180# coated asphalt in anhydrous ethanol at a mass ratio of 1:1:2, and the solid content of the mixed carbon source slurry was 35% (mass fraction), wherein the diameter of the carbon tubes was a single-arm carbon tube with a diameter of 3~20nm; after filtration and drying, it was calcined at 650°C in an argon atmosphere for 4.5 hours to obtain a finished product I with a particle size of 5μm, i.e., a fast-charging and long-cycle silicon-carbon negative electrode material.

[0038] The obtained fast-charge and long-cycle silicon-carbon negative electrode material and metal lithium sheet were used to form a CR2032 half-cell for electrochemical performance testing. The assembly order was negative electrode shell, metal lithium sheet, diaphragm, fast-charge and long-cycle silicon-carbon negative electrode material electrode sheet, gasket, and positive electrode shell. The electrolyte added was Xinzhoubang LBC3021H43. The test rate was 0.1C (first time) + 0.5C (cycle). The results showed that the discharge specific capacity of the negative electrode sheet could reach 1696mAh / g, with an initial efficiency of 82.1%. After 50 cycles, the capacity could still be maintained at 83.2%.

[0039] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, electrode ear welding, top and side sealing, baking, and liquid injection (Xinzhoubang LBC3021H43) were carried out to assemble 7Ah soft-pack batteries. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The initial efficiency of the battery cell was 86.5%. After 647 weeks of full battery cycling, the capacity retention rate was 84.7%.

[0040] Example 4 (1) Dispersing single-arm carbon nanotubes with a diameter of 0.9 nm and a length of 15 nm in anhydrous ethanol to form a solution with a solid content of 4% (mass fraction), and then adding a 36% mass fraction formaldehyde solution, with a mass ratio of single-arm carbon nanotubes to formaldehyde of 1:60, to obtain solution B; (2) Bisphenol A was heated to 170°C, then added to solution B and stirred. The mass ratio of bisphenol A to solution B was 1:7. The resulting solution was heated to 190°C, and 0.5 mol / L sodium carbonate solution was added dropwise to adjust the pH of the solution to 9.5. The solution was stopped when solid began to appear, and stirring was continued until it was completely solidified to obtain solid C. Solid C was then crushed into block particles with a particle size of 3 μm to obtain carbon precursor D. (3) The carbon precursor D and lithium hydroxide were mixed evenly in a mass ratio of 1:3, and calcined at 800 °C for 3 h under a nitrogen atmosphere to obtain a mixture E; then the mixture was placed in a 0.2 mol / L hydrochloric acid solution and stirred for 20 min, wherein the mass ratio of the mixture E to the hydrochloric acid solution was 1:4; after drying, the mixture was washed with distilled water for multiple times until the solution pH was ≤8. After drying, the pore size was 2 nm and the specific surface area was 2100 m 2 / g, and the pore volume is 0.93 cc / g porous carbon matrix F; (4) The porous carbon substrate F was placed in a fluidized bed, and a mixture of monosilane and nitrogen was introduced at a volume ratio of 1:4, heated to 600°C and kept warm for 4 hours, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:2, and kept warm at 700°C for 3 hours to obtain product G; (5) Product G was placed in a chemical vapor deposition furnace, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:2, and the mixture was kept at 700°C for 3.5 hours to obtain product H; then it was placed in a mixed carbon source slurry, and the mass ratio of product H to the mixed carbon source slurry was 10:1, wherein the mixed carbon source slurry was obtained by dispersing graphene, carbon tubes and Xinjiang Zhongtan 150# coated asphalt in anhydrous ethanol at a mass ratio of 1:1:2, and the solid content of the mixed carbon source slurry was 35% (mass fraction), wherein the diameter of the carbon tubes was a single-arm carbon tube with a diameter of 3~20nm; after filtration and drying, it was calcined at 800°C in an argon atmosphere for 5.5 hours to obtain a finished product I with a particle size of 8μm, i.e., a fast-charging and long-cycle silicon-carbon negative electrode material.

[0041] The obtained fast-charging and long-cycle silicon-carbon negative electrode material and metal lithium sheet were used to form a CR2032 half-cell for electrochemical performance testing. The assembly order was negative electrode shell, metal lithium sheet, diaphragm, fast-charging and long-cycle silicon-carbon negative electrode material electrode sheet, gasket, and positive electrode shell. The electrolyte added was Xinzhoubang LBC3021H43. The test rate was 0.1C (first time) + 0.5C (cycle). The results showed that the discharge specific capacity of the negative electrode sheet could reach 1600 mAh / g, with an initial efficiency of 82.8%. After 50 cycles, it could still maintain 84.9% of the capacity.

[0042] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection (Xinzhoubang LBC3021H43) were carried out to assemble 7Ah soft-pack batteries. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The initial efficiency of the battery cell was 87.4%. After 450 cycles of the full battery, the capacity retention rate was 94.1%.

[0043] Example 5 (1) Dispersing single-arm carbon nanotubes with a diameter of 1 nm and a length of 20 nm in anhydrous ethanol to form a solution with a solid content of 5% (mass fraction), and then adding a 36% formaldehyde solution with a mass ratio of single-arm carbon nanotubes to formaldehyde of 1:80 to obtain solution B; (2) Bisphenol A was heated to 170°C, added to solution B and stirred, the mass ratio of bisphenol A to solution B was 1:8, the resulting solution was heated to 200°C, 0.5 mol / L sodium carbonate solution was added dropwise to adjust the pH of the solution to 10, and the solution was stopped when solid began to appear, and stirring was continued until it was completely solidified to obtain solid C; solid C was then crushed into block particles with a particle size of 4 μm to obtain carbon precursor D; (3) The carbon precursor D and lithium hydroxide were mixed evenly in a mass ratio of 1:4, and calcined at 900 °C for 5 h under a nitrogen atmosphere to obtain a mixture E; then the mixture was placed in a 0.2 mol / L hydrochloric acid solution and stirred for 20 min, wherein the mass ratio of the mixture E to the hydrochloric acid solution was 1:5; after drying, the mixture was washed with distilled water for multiple times until the solution pH was ≤8. After drying, the pore size was 3 nm and the specific surface area was 2200 m 2 / g, pore volume is 1.0 cc / g porous carbon matrix F; (4) The porous carbon substrate F was placed in a fluidized bed, and a mixture of monosilane and nitrogen was introduced at a volume ratio of 1:5, heated to 700°C and kept warm for 6 hours, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:3, and kept warm at 750°C for 3 hours to obtain product G; (5) Product G was placed in a chemical vapor deposition furnace, and a mixture of acetylene and argon was introduced at a gas flow ratio of 1:2, and the mixture was kept at 750°C for 4 hours to obtain product H; then it was placed in a mixed carbon source slurry, the mass ratio of product H to the mixed carbon source slurry was 10:1, wherein the mixed carbon source slurry was obtained by dispersing graphene, carbon tubes and Xinjiang Zhongtan 180# coated asphalt in anhydrous ethanol at a mass ratio of 1:1:2, and the solid content of the mixed carbon source slurry was 35% (mass fraction), wherein the diameter of the carbon tubes was a single-arm carbon tube with a diameter of 3~20nm; after filtration and drying, it was calcined at 900°C in an argon atmosphere for 6 hours to obtain a finished product I with a particle size of 10μm, i.e., a fast-charging and long-cycle silicon-carbon negative electrode material.

[0044] The obtained fast-charge and long-cycle silicon-carbon negative electrode material and metal lithium sheet were used to form a CR2032 half-cell for electrochemical performance testing. The assembly order was negative electrode shell, metal lithium sheet, diaphragm, fast-charge and long-cycle silicon-carbon negative electrode material electrode sheet, gasket, and positive electrode shell. The electrolyte added was Xinzhoubang LBC3021H43. The test rate was 0.1C (first time) + 0.5C (cycle). The results showed that the discharge specific capacity of the negative electrode sheet could reach 1580 mAh / g, with an initial efficiency of 82.0%. After 50 cycles, 83.1% of the capacity could still be maintained.

[0045] The obtained long-cycle silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection (Xinzhoubang LBC3021H43) were carried out to assemble 7Ah soft-pack batteries. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The initial efficiency of the battery cell was 87.2%. After 450 cycles of the full battery, the capacity retention rate was 92.5%.

[0046] Comparative Example 1 The porous carbon matrix (pore size 2.2nm, specific surface area 1800m) of Shaanxi Coal Technology Research Institute with D50 of 8μm 2 / g, pore volume of 0.8 cc / g), put it into a fluidized bed, introduce a mixed gas of silane and hydrogen at a gas flow volume ratio of 2:1, heat to 700℃ and keep warm for 6h, then introduce a mixed gas of acetylene and argon at a gas flow ratio of 1:3, and keep warm at 750℃ for 3h to obtain a silicon-carbon negative electrode material.

[0047] The silicon-carbon negative electrode material obtained in this comparative example and metal lithium formed a half-cell for electrochemical performance testing (the same as Example 1), with a test rate of 0.1C (first time) + 0.5C (cycle), and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge specific capacity of the negative electrode sheet could reach 1580 mAh / g, with an initial efficiency of 82.0%, and after 50 cycles, it could still maintain 51.1% of the capacity.

[0048] It can be seen from the performance results of the embodiments that the present invention uses a small-sized core ((1~3μm porous carbon matrix F) to deposit nanosilicon, shorten the lithium ion transmission particle size, and then granulate and surface modify the core by mixing the carbon source slurry, compound one or more cores to form a slightly larger finished product, and through the core composite single-arm carbon tube, connect each pore of the core, improve the fast channel of ion and electron transport, improve the material rate performance, form a "rebar-cement" type structure, increase the structural strength of the core, increase the material's anti-expansion property, and improve the electrochemical performance. The graphene and carbon tubes mixed with the carbon source slurry form a "rebar-cement" type structure in the outer coating layer, forming a high structural strength material, while having excellent electrical conductivity and high rate capability.

Claims

1. A method for preparing a silicon-carbon negative electrode material, comprising the following steps: (1) dispersing the single-arm carbon nanotubes in a solvent to obtain a solution A; and then mixing the solution A with a formaldehyde solution to obtain a solution B; (2) dissolving bisphenol A in the solution B, heating it, and then adding a catalyst to adjust the pH of the solution to 7-10, so that the solution is completely solidified to obtain a solid C; crushing the solid C to obtain a carbon precursor D; (3) mixing the carbon precursor D and the alkaline activator, calcining, and obtaining a mixture E; washing the mixture E, and obtaining a porous carbon matrix F; (4) placing the porous carbon substrate F into a fluidized bed, introducing a mixed gas of silane and nitrogen, and heating and keeping the temperature; then introducing a mixed gas of acetylene and argon, and heating and keeping the temperature, to obtain product G; (5) Depositing carbon on the surface of product G by chemical vapor deposition to obtain product H; (6) The product H is mixed with a mixed carbon source slurry, and calcined to obtain the silicon-carbon negative electrode material.

2. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: In step (1), the diameter of the single-arm carbon tube is 0.5-1 nm, and the length is 2-20 nm; The solvent is anhydrous ethanol; In the solution A, the solid content of the single-arm carbon tube is 0.5% to 5%; The mass percentage concentration of the formaldehyde solution is 35% to 37%; The mass ratio of the single-arm carbon tube to formaldehyde is 1:35-80; In step (2), the mass ratio of bisphenol A to solution B is 1:5-8; The catalyst is at least one of a sodium carbonate solution, a sodium hydroxide solution and an ammonium hydroxide solution; The solid C is crushed into block particles with a particle size of 1-4 μm, which is the carbon precursor D.

3. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The specific operation of step (2) is as follows: dissolving bisphenol A in the solution B, heating the resulting solution to 180-200° C., then dropping a catalyst to adjust the solution pH to 7-10, stopping when solid begins to appear in the solution, and continuing stirring until it is completely solidified to obtain a solid C; crushing the solid C to obtain a carbon precursor D.

4. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: In step (3), the alkaline activator is at least one of potassium hydroxide, sodium hydroxide and lithium hydroxide; The mass ratio of the carbon precursor D to the alkaline activator is 1:1-4; The calcination is carried out in an inert atmosphere; The calcination temperature is 700-900°C; the calcination time is 1-5h; The washing is carried out using a hydrochloric acid solution and water in sequence; specifically, the concentration of the hydrochloric acid is 0.1-2 mol / L.

5. The method for preparing the silicon-carbon negative electrode material according to claim 4, characterized in that: In step (3), the washing operation is as follows: placing the mixture E in a hydrochloric acid solution and stirring and washing for 10 to 60 minutes, and then washing with water for multiple times until the solution pH is ≤8; Specifically, the mass ratio of the mixture E to the hydrochloric acid solution may be 1:2-5.

6. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The specific operation of step (4) is as follows: the porous carbon substrate F is placed in a fluidized bed, a silane and nitrogen mixture with a volume ratio of 5:1 to 1:5 is introduced, and the temperature is kept at 400 to 700° C. for 2 to 6 hours; then, a acetylene and argon mixture with a gas flow ratio of 2:1 to 1:3 is introduced, and the temperature is kept at 650 to 750° C. for 1 to 3 hours to obtain product G; The silane is one of monosilane or disilane.

7. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The specific operation of step (5) is as follows: placing the product G in a chemical vapor deposition reactor, introducing a mixture of acetylene and argon at a gas flow ratio of 2:1 to 1:2, and maintaining the temperature at 650 to 750° C. for 1 to 4 hours to obtain product H.

8. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: Step (6), the mass ratio of the product H to the mixed carbon source slurry is 10:1 to 15:1; The mixed carbon source slurry is obtained by dispersing graphene, carbon tubes and low-temperature asphalt in anhydrous ethanol; specifically, the mass ratio of the graphene, carbon tubes and low-temperature asphalt can be 1:1:2; the solid content of the mixed carbon source slurry can be 30% to 40%; the carbon tubes are single-arm carbon tubes with a tube diameter of 3 to 20 nm; The calcination is carried out in an inert atmosphere; The calcination temperature is 600-900° C. and the calcination time is 4-6 hours.

9. The silicon-carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the silicon-carbon negative electrode material according to claim 9 in preparing a negative electrode for a lithium-ion battery.

Citation Information

Patent Citations

  • Silicon and carbon negative electrode material for lithium ion battery and preparation method thereof

    CN109671942A

  • Silicon-carbon composite negative electrode material and preparation method thereof

    CN115663132A

  • Fast-charging graphite composite material as well as preparation method and application thereof

    CN116646489A

  • Carbon nanotube-containing silicon-carbon composite material as well as preparation method and application thereof

    CN116995206A

  • Pre-lithiated silicon-carbon multilayer composite negative electrode material for lithium ion batteries and preparation method thereof

    US20220216477A1

Cited By

  • High-capacity silicon-carbon negative electrode material and preparation process thereof

    CN120261548A