Geopolymer grouting reinforcement material and preparation method thereof

By using geopolymer grouting materials prepared from raw materials such as silicon-aluminum source powder and alkaline activators, the problem of insufficient mechanical properties of existing grouting materials has been solved, and the goals of efficient reinforcement and environmental protection of coal mine surrounding rocks have been achieved.

CN118771791AInactive Publication Date: 2024-10-15GENERAL PROSPECTING INSTITUTE OF CHINA NATIONAL ADMINISTRATION OF COAL GEOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410817481.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing grouting materials have insufficient mechanical properties in the field of coal mines, cannot effectively reinforce small pores and cracks, and have environmental protection and cost issues.

Method used

Geopolymer grouting reinforcement materials prepared from silicon-aluminum source powder, alkaline activators, admixtures and water are used to improve material performance through calcination and alkali activation reactions. Raw materials such as coal gangue and waste glass are used to reduce costs and environmental impact. .

Benefits of technology

The prepared geopolymer grouting reinforcement material has excellent mechanical properties and can effectively reinforce the coal mine surrounding rock, meet the application needs of the coal mining industry, reduce project costs and achieve environmental protection goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910681390000091
    Figure BDA0004910681390000091
  • Figure BDA0004910681390000101
    Figure BDA0004910681390000101
Patent Text Reader

Abstract

The invention belongs to the technical field of grouting reinforcement materials, and provides a geopolymer grouting reinforcement material and a preparation method thereof. The preparation method comprises the following steps: S1, calcining silicon-aluminum source powder to obtain activated silicon-aluminum source powder; s2, mixing the activated silicon-aluminum source powder, an alkaline activator and water, and reacting to obtain a crude product; and S3, mixing the crude product with an additive to obtain the geopolymer grouting reinforcement material. The geopolymer grouting reinforcement material is prepared by taking solid wastes such as waste glass and coal gangue as main raw materials, so that the problem of solid waste stacking can be solved, a large amount of land resources are saved, and the prepared geopolymer grouting reinforcement material is excellent in comprehensive performance, can meet the application requirements of surrounding rock reinforcement in the coal mine industry, and has a wide application prospect. Wide popularization and application prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grouting reinforcement materials, and in particular to a geopolymer grouting reinforcement material and a preparation method thereof. Background Art

[0002] In the process of coal mine production, it is common to encounter phenomena such as tunnel surrounding rock crushing and roof cracking caused by stress concentration. The stress on the coal wall in the coal tunnel will cause the structural strength and stability of the coal wall to decrease, which is not conducive to tunnel support and affects safe production. Grouting is usually used to reinforce the surrounding rock. At present, grouting materials are mainly divided into cement slurry and chemical slurry. Cement grouting materials have the advantages of low cost, abundant sources of raw materials and convenient slurry configuration, but cement slurry has the disadvantages of poor fluidity and long setting time. This slurry is generally only suitable for injection into pores or cracks with a diameter or width of ≥0.2mm, and is subject to certain restrictions in engineering applications. Chemical grouting materials have the advantages of low slurry viscosity, good injectability, and can be injected into small cracks, but they are expensive and have certain toxicity, posing a certain threat to people's lives and health.

[0003] Geopolymer is an inorganic polymer with a three-dimensional network structure composed of AlO4 and SiO4 tetrahedral structural units. It has the characteristics of high strength, high fluidity, good permeability, good construction performance and durability. Using geopolymer as grouting material has two major advantages: (1) The raw materials of geopolymer are widely available and low in cost, which can effectively reduce the cost of grouting projects; (2) Compared with cement materials, geopolymer materials have the advantages of low energy consumption and green environmental protection, which can realize the effective recycling and reuse of industrial waste residues and reduce large amounts of CO2 emissions, and have far-reaching environmental and social benefits.

[0004] Due to the particularity of the coal mining field, there are also high requirements for the mechanical properties of the consolidated body after grouting reinforcement. Therefore, how to prepare a geopolymer grouting reinforcement material with excellent mechanical properties has become a problem that technicians in this field need to solve urgently. Summary of the invention

[0005] In view of this, the present invention provides a geopolymer grouting reinforcement material and a preparation method thereof, the purpose of which is to solve the technical problem of insufficient mechanical properties of existing grouting materials.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention provides a geopolymer grouting reinforcement material, which is prepared from the following raw materials:

[0008] Silica and aluminum source powder, alkaline activator, additives and water;

[0009] The amount of the alkaline activator is 1-20% of the mass of the silicon-aluminum source powder, the amount of the admixture is 1-10% of the mass of the silicon-aluminum source, and the amount of water is 30-50% of the mass of the silicon-aluminum source powder;

[0010] The silicon-aluminum source powder comprises the following components in parts by weight: 30-40 parts of coal gangue, 20-40 parts of waste glass, 10-20 parts of steel slag, 10-20 parts of metakaolin, and 10-20 parts of fly ash.

[0011] Furthermore, the alkaline activator includes one or more of water glass, KOH, NaOH, Ca(OH)2, K2SO4, Na2SO4 and CaSO4.

[0012] Furthermore, the particle sizes of the coal gangue, steel slag, metakaolin and fly ash are all ≤0.5 mm; and the waste glass includes three powder states of 30-50 μm, 70-150 μm and 200-300 μm.

[0013] Furthermore, the admixture includes one or more of an expansion agent, a water reducing agent and an accelerating setting agent.

[0014] Furthermore, the expansion agent includes one or more of magnesium oxide, calcium oxide and calcium sulphoaluminate.

[0015] Furthermore, the water reducer includes a polycarboxylate water reducer or a naphthalene water reducer.

[0016] Furthermore, the accelerating setting agent includes polyacrylic acid and / or polymethacrylic acid.

[0017] The present invention also provides a method for preparing the above-mentioned geopolymer grouting reinforcement material, comprising the following steps:

[0018] S1, calcining the silicon-aluminum source powder to obtain activated silicon-aluminum source powder;

[0019] S2, mixing the activated silicon-aluminum source powder, alkaline activator and water and reacting them to obtain a crude product;

[0020] S3. The crude product is mixed with an admixture to obtain a geopolymer grouting reinforcement material.

[0021] Furthermore, in step S1, the calcination temperature is 800-1200° C., and the calcination time is 1-5 hours.

[0022] Furthermore, in step S2, the reaction temperature is 40-100° C., and the reaction time is 30-60 min.

[0023] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:

[0024] Coal gangue is an inevitable product of coal mining production, and waste glass is a solid waste that is difficult to utilize. The present invention uses coal gangue and waste glass as main raw materials, which can not only solve the problem of solid waste stacking and save a lot of land resources, but also the prepared geopolymer grouting reinforcement material has excellent comprehensive performance and can meet the application needs of surrounding rock reinforcement in the coal mining industry.

[0025] For most active silicon-aluminum source materials, the use of calcination heat activation has little effect on the properties of the raw materials. The present invention improves the reaction activity of the raw materials by regulating the fineness of the raw materials and the calcination temperature. In the subsequent alkali excitation process, the difficulty of alkali excitation is reduced, and the active substances in the silicon-aluminum source materials are leached, thereby improving the performance of the geopolymer grouting reinforcement material. DETAILED DESCRIPTION

[0026] The present invention provides a geopolymer grouting reinforcement material, which is prepared from the following raw materials:

[0027] Silica and aluminum source powder, alkaline activator, additives and water;

[0028] The amount of the alkaline activator used is 1-20% of the mass of the silicon-aluminum source powder, preferably 3-16%, and more preferably 6-12%; the amount of the admixture used is 1-10% of the mass of the silicon-aluminum source, preferably 2-8%, and more preferably 4-6%; the amount of water used is 30-50% of the mass of the silicon-aluminum source powder, preferably 35-45%, and more preferably 40%.

[0029] In the present invention, the silicon-aluminum source powder comprises the following components in parts by weight: 30-40 parts of coal gangue, 20-40 parts of waste glass, 10-20 parts of steel slag, 10-20 parts of metakaolin, and 10-20 parts of fly ash.

[0030] In the present invention, the amount of coal gangue used is preferably 32 to 38 parts, and more preferably 34 to 36 parts.

[0031] In the present invention, the amount of waste glass used is preferably 24 to 36 parts, more preferably 28 to 32 parts.

[0032] In the present invention, the amount of steel slag used is preferably 12 to 18 parts, more preferably 14 to 16 parts.

[0033] In the present invention, the amount of metakaolin used is preferably 12 to 18 parts, more preferably 14 to 16 parts.

[0034] In the present invention, the amount of fly ash used is preferably 12 to 18 parts, more preferably 14 to 16 parts.

[0035] In the present invention, the content of SiO2+Al2O3 in the waste glass is ≥70%, preferably ≥72%, and more preferably ≥75%.

[0036] In the present invention, the alkaline activator includes one or more of water glass, KOH, NaOH, Ca(OH)2, K2SO4, Na2SO4 and CaSO4, preferably one or more of water glass, KOH, NaOH, K2SO4 and Na2SO4, and further preferably one or more of water glass, KOH and NaOH.

[0037] In the present invention, the particle sizes of the coal gangue, steel slag, metakaolin and fly ash are all ≤0.5mm, preferably ≤0.4mm, and more preferably ≤0.3mm; the waste glass comprises three powder states of 30-50μm, 70-150μm and 200-300μm, preferably comprises three powder states of 34-48μm, 80-140μm and 220-280μm, and more preferably comprises three powder states of 38-46μm, 90-120μm and 240-260μm; the waste glass in the three powder states is preferably of equal quality.

[0038] In the present invention, the admixture includes one or more of an expansive agent, a water reducing agent and an accelerator, preferably an expansive agent, a water reducing agent and an accelerator are used together.

[0039] In the present invention, the expansion agent includes one or more of magnesium oxide, calcium oxide and calcium sulfoaluminate, preferably magnesium oxide and / or calcium oxide, and more preferably magnesium oxide.

[0040] In the present invention, the water reducer includes a polycarboxylate water reducer or a naphthalene water reducer, preferably a polycarboxylate water reducer.

[0041] In the present invention, the accelerating setting agent comprises polyacrylic acid and / or polymethacrylic acid, preferably polyacrylic acid.

[0042] The present invention also provides a method for preparing the above-mentioned geopolymer grouting reinforcement material, comprising the following steps:

[0043] S1, calcining the silicon-aluminum source powder to obtain activated silicon-aluminum source powder;

[0044] S2, mixing the activated silicon-aluminum source powder, alkaline activator and water and reacting them to obtain a crude product;

[0045] S3. The crude product is mixed with an admixture to obtain a geopolymer grouting reinforcement material.

[0046] In the present invention, in step S1, the calcination temperature is 800-1200°C, preferably 850-1150°C, and more preferably 900-1100°C; the calcination time is 1-5h, preferably 2-4h, and more preferably 3h.

[0047] In the present invention, in step S2, the reaction temperature is 40-100°C, preferably 50-90°C, and more preferably 60-80°C; the reaction time is 30-60 min, preferably 40-50 min, and more preferably 45 min.

[0048] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0049] Example 1

[0050] The steel slag, coal gangue and waste glass were preliminarily crushed by a pulverizer, and ball-milled for 10 minutes by a ball mill (1000 rpm). The steel slag and coal gangue were sieved, and powders with a particle size of ≤0.5 mm were used for later use; the waste glass powder was screened according to small particle size (30-50 μm), medium particle size (70-150 μm) and large particle size (200-300 μm) for later use; the fly ash and metakaolin were ground and sieved, and powders with a particle size of ≤0.5 mm were used for later use.

[0051] Take 30 parts of coal gangue, 30 parts of waste glass (10 parts each of large, medium and small particle sizes), 10 parts of steel slag, 10 parts of metakaolin and 20 parts of fly ash, mix them, heat them to 900°C in a muffle furnace, and calcine them for 4 hours to obtain activated silicon-aluminum source powder.

[0052] Take 9 parts of alkaline activator (3 parts each of water glass, KOH and NaOH) and mix them with 40 parts of water to obtain an alkaline activator solution, put the activated silicon aluminum source powder into the alkaline activator solution, and react at 60°C for 50 minutes to obtain a crude product; 3 parts of magnesium oxide, 2 parts of polycarboxylic acid water reducer, and 1 part of polyacrylic acid are mixed evenly with the crude product to obtain a geopolymer grouting reinforcement material.

[0053] Example 2

[0054] The steel slag, coal gangue and waste glass were preliminarily crushed by using a crusher, and were ball-milled for 10 minutes by using a ball mill (1000rpm). The steel slag and coal gangue were sieved respectively, and powders with a particle size of ≤0.5mm were used for later use; the waste glass powder was screened according to small particle size (35-45μm), medium particle size (80-140μm) and large particle size (220-280μm) for later use; the fly ash and metakaolin were ground and sieved respectively, and powders with a particle size of ≤0.5mm were used for later use.

[0055] Take 35 parts of coal gangue, 33 parts of waste glass (11 parts each of large, medium and small particle sizes), 12 parts of steel slag, 10 parts of metakaolin and 10 parts of fly ash, mix them, heat them to 1000°C in a muffle furnace, and calcine them for 3 hours to obtain activated silicon-aluminum source powder.

[0056] Take 12 parts of alkaline activator (4 parts each of water glass, Ca(OH)2 and CaSO4) and mix them with 45 parts of water to obtain an alkaline activator solution, put the activated silicon aluminum source powder into the alkaline activator solution, and react at 70°C for 40 minutes to obtain a crude product; 3 parts of calcium oxide, 3 parts of naphthalene-based water reducer, and 1 part of polymethacrylic acid are mixed evenly with the crude product to obtain a geopolymer grouting reinforcement material.

[0057] Example 3

[0058] The steel slag, coal gangue and waste glass were preliminarily crushed by a pulverizer, and ball-milled for 15 minutes by a ball mill (1000rpm). The steel slag and coal gangue were sieved respectively, and powders with a particle size of ≤0.5mm were used for later use; the waste glass powder was screened according to small particle size (32-48μm), medium particle size (90-120μm) and large particle size (240-260μm) for later use; the fly ash and metakaolin were ground and sieved respectively, and powders with a particle size of ≤0.5mm were used for later use.

[0059] Take 40 parts of coal gangue, 24 parts of waste glass (8 parts each of large, medium and small particle sizes), 12 parts of steel slag, 12 parts of metakaolin and 12 parts of fly ash, mix them, heat them to 1100°C in a muffle furnace, and calcine them for 1.5 hours to obtain activated silicon-aluminum source powder.

[0060] Take 15 parts of alkaline activator (5 parts each of water glass, K2SO4 and Na2SO4) and mix them with 50 parts of water to obtain an alkaline activator solution, put the activated silicon aluminum source powder into the alkaline activator solution, and react at 45°C for 60 minutes to obtain a crude product; 1 part of calcium sulfoaluminate, 2 parts of naphthalene-based water reducer, and 3 parts of polymethacrylic acid are mixed evenly with the crude product to obtain a geopolymer grouting reinforcement material.

[0061] Comparative Example 1

[0062] The same as Example 1, except that the calcination temperature is 600° C. and the calcination time is 8 h.

[0063] Comparative Example 2

[0064] The same as Example 1, except that the particle sizes of coal gangue, steel slag, metakaolin and fly ash are all selected to be powders between 1 and 5 mm.

[0065] Comparative Example 3

[0066] The same as Example 1, except that the particle size of the waste glass only includes powders between 70 and 150 μm.

[0067] According to the standard AQ1089-2011 "Polymer materials for reinforcing coal and rock masses in coal mines", the performance of the geopolymer grouting reinforcement materials obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was measured, and the measurement results are shown in Table 1.

[0068] Table 1 Performance test results of geopolymer grouting reinforcement materials

[0069]

[0070]

[0071] As shown in Table 1, the calcination temperature and the particle size of the raw materials have an important influence on the activation of the raw materials, thereby affecting the performance of the geopolymer grouting reinforcement material. The use of metakaolin increases the viscosity of the geopolymer grouting reinforcement material, shortens the curing time, and improves the solidification rate. The use of waste glass of different particle sizes further improves the fluidity of the geopolymer grouting reinforcement material, making the solidified geopolymer grouting reinforcement material more compact and having better bonding strength. At the same time, waste glass of different particle sizes can also fill pores of different particle sizes, enhance the density of the geopolymer grouting reinforcement material, and thus enhance its mechanical properties.

[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A geopolymer grouting reinforcement material, characterized in that: Prepared from the following raw materials: Silica and aluminum source powder, alkaline activator, additives and water; The amount of the alkaline activator is 1-20% of the mass of the silicon-aluminum source powder, the amount of the admixture is 1-10% of the mass of the silicon-aluminum source, and the amount of water is 30-50% of the mass of the silicon-aluminum source powder; The silicon-aluminum source powder comprises the following components in parts by weight: 30-40 parts of coal gangue, 20-40 parts of waste glass, 10-20 parts of steel slag, 10-20 parts of metakaolin, and 10-20 parts of fly ash.

2. The geopolymer grouting reinforcement material according to claim 1, characterized in that: The alkaline activator includes one or more of water glass, KOH, NaOH, Ca(OH)2, K2SO4, Na2SO4 and CaSO4.

3. The geopolymer grouting reinforcement material according to claim 2, characterized in that: The particle sizes of the coal gangue, steel slag, metakaolin and fly ash are all less than or equal to 0.5 mm; the waste glass includes three powder states of 30-50 μm, 70-150 μm and 200-300 μm.

4. The geopolymer grouting reinforcement material according to any one of claims 1 to 3, characterized in that: The admixture includes one or more of an expansion agent, a water reducing agent and an accelerating setting agent.

5. The geopolymer grouting reinforcement material according to claim 4, characterized in that: The expansion agent includes one or more of magnesium oxide, calcium oxide and calcium sulphoaluminate.

6. The geopolymer grouting reinforcement material according to claim 5, characterized in that: The water reducer includes a polycarboxylate water reducer or a naphthalene water reducer.

7. The geopolymer grouting reinforcement material according to claim 5 or 6, characterized in that: The quick-setting agent includes polyacrylic acid and / or polymethacrylic acid.

8. The method for preparing the geopolymer grouting reinforcement material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, calcining the silicon-aluminum source powder to obtain activated silicon-aluminum source powder; S2, mixing the activated silicon-aluminum source powder, alkaline activator and water and reacting them to obtain a crude product; S3. The crude product is mixed with an admixture to obtain a geopolymer grouting reinforcement material.

9. The preparation method according to claim 8, characterized in that: In the step S1, the calcination temperature is 800-1200° C., and the calcination time is 1-5 hours.

10. The preparation method according to claim 9, characterized in that: In step S2, the reaction temperature is 40-100° C., and the reaction time is 30-60 min.