Performance regulation and control method for geopolymer dry powder material

Through the combination adjustment of different silicon-aluminum ratios and calcining temperatures, geological polymer dry powder materials are prepared, which solves the shortcomings in the regulation of geological polymer coagulation time and strength in the prior art, and improves its application in construction engineering materials.

CN118993591AActive Publication Date: 2024-11-22CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202410980115.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-22
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The existing geological polymer preparation methods have shortcomings in regulating the settling time and strength, and further improvements are needed to meet engineering requirements.

Method used

Silicon-aluminum raw materials with different silicon-aluminum ratios are mixed with alkaline substances, divided into high-temperature, medium-temperature and low-temperature roasting, and 9 kinds of roasting materials are prepared, and appropriate roasting materials and gel-active silicon-aluminum raw materials are selected according to the performance of the required geological polymer. Mix, control the silicon-aluminum ratio and calcining temperature to regulate the performance of the geological polymer.

Benefits of technology

By adjusting the silicon-aluminum ratio and calcining temperature, the reaction process and performance of geological polymers can be effectively regulated and its application in the field of construction engineering materials can be improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993591A_ABST
    Figure CN118993591A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of geopolymer preparation, in particular to a geopolymer dry powder material performance regulation and control method. The method comprises the following steps: firstly, classifying silicon-aluminum raw materials according to high, medium and low silicon-aluminum ratios, mixing the classified silicon-aluminum raw materials with an alkaline substance, then classifying, and respectively carrying out high-temperature roasting, medium-temperature roasting and low-temperature roasting on the classified materials to finally obtain nine roasted materials with different silicon-aluminum ratios and roasting temperatures; selecting any 1-9 roasting materials according to the compressive strength of the geopolymer to be prepared, and mixing to obtain a mixed roasting material; and mixing the roasted material with a gel active silicon-aluminum raw material, and grinding to obtain the required geopolymer dry powder material. According to the present invention, the silica-alumina ratio of the silica-alumina raw material and the alkali fusion thermal activation temperature are adjusted so as to adjust the phase of the roasting product, such that the geopolymer reaction process regulation and control method is formed, and the applicability of the geopolymer in the fields of construction engineering materials and the like can be substantially improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of geopolymer preparation, and in particular to a method for controlling the performance of geopolymer dry powder materials. Background Art

[0002] Geopolymer is an inorganic gelling material with the advantages of early strength and fast hardening, chemical corrosion resistance, good durability, rich synthetic raw materials, and low carbon emissions. Therefore, it is regarded as a new type of building material after lime and silicate cement. In recent years, geopolymer has attracted widespread attention from countries around the world. Studies have shown that it has broad application and development prospects in the fields of building materials, sealing materials and solid waste disposal.

[0003] The large-scale application of geopolymers needs to meet various engineering requirements, so the performance control of geopolymers is one of the keys to its promotion and application. In order to optimize the preparation method and performance control of geopolymers, the applicant's previous patent CN113003968A disclosed a geopolymer dry powder material and its preparation method, which uses the mixing of alkali-melting materials and active materials to achieve the water-adding preparation of geopolymers, which can solve the problem of liquid alkali-excited preparation in the prior art to a certain extent; Patent CN116514426A further proposed a preparation method of homogenized geopolymer dry powder, which improves the performance of geopolymers by controlling the chemical homogeneity of the material.

[0004] However, the above two patents mainly focus on the regulation of roasting materials at the same temperature. In order to better control the coagulation time, strength and other properties of geopolymers, the coupling of roasting temperature and raw material properties needs to be considered in actual preparation. Therefore, it is necessary to further improve the existing preparation method. Summary of the invention

[0005] In order to solve the above problems, the present invention first provides a method for controlling the properties of geopolymer dry powder materials.

[0006] The present invention adopts the following technical solutions:

[0007] A method for controlling the performance of a geopolymer dry powder material comprises the following steps:

[0008] S1. Preparation of roasting materials

[0009] S11. Confirm the classification of silicon-aluminum raw materials: the silicon-aluminum raw materials include high silicon-aluminum ratio, medium silicon-aluminum ratio, and low silicon-aluminum ratio. The silicon-aluminum ratio of the high silicon-aluminum ratio is greater than or equal to 15, the silicon-aluminum ratio of the medium silicon-aluminum ratio is 6-10, and the silicon-aluminum ratio of the low silicon-aluminum ratio is 1-6;

[0010] S12. The silicon-aluminum raw material is mixed with an alkaline substance in a set ratio, and the mixed material is divided into three parts according to a set ratio, and high-temperature roasting, medium-temperature roasting, and low-temperature roasting are performed respectively, wherein the high-temperature roasting temperature is 600 to 700 ° C, the medium-temperature roasting temperature is 400 to 600 ° C, and the low-temperature roasting temperature is 250 to 400 ° C;

[0011] Thus, 9 kinds of roasting materials are obtained, namely, high silicon-aluminum ratio-high temperature material, high silicon-aluminum ratio-medium temperature material, high silicon-aluminum ratio-low temperature material, medium silicon-aluminum ratio-high temperature material, medium silicon-aluminum ratio-medium temperature material, medium silicon-aluminum ratio-low temperature material, low silicon-aluminum ratio-high temperature material, low silicon-aluminum ratio-medium temperature material, and low silicon-aluminum ratio-low temperature material;

[0012] S2. Preparation of geopolymers

[0013] S21. According to the compressive strength of the geopolymer to be prepared, any 1 to 9 of the 9 calcined materials are selected and mixed to obtain a mixed calcined material;

[0014] S22. The mixed roasted material and the gel active silica-alumina raw material are mixed in a mass ratio of (0.10-0.25):1 to obtain a mixed material, and the silica-alumina ratio of the gel active silica-alumina raw material is controlled so that the silica-alumina ratio of the mixed material is 2-5. The mixed material is ground to obtain the desired geopolymer dry powder material.

[0015] Preferably, the mixing strategy of the 9 kinds of roasting materials is: sorted by the weight of influence on compressive strength, in order: medium silicon-aluminum ratio-medium temperature material, medium silicon-aluminum ratio-low temperature material, medium silicon-aluminum ratio-high temperature material, high silicon-aluminum ratio-medium temperature material, high silicon-aluminum ratio-low temperature material, high silicon-aluminum ratio-high temperature material, low silicon-aluminum ratio-medium temperature material, low silicon-aluminum ratio-low temperature material, low silicon-aluminum ratio-high temperature material, and medium silicon-aluminum ratio-medium temperature material is a positive condition for enhancing the compressive strength, and low silicon-aluminum ratio-high temperature material is a positive condition for reducing the compressive strength, and as the silicon-aluminum ratio of the roasting material decreases, the solidification time of the slurry is shortened.

[0016] Preferably, the silicon-aluminum raw material is one or more of coal gangue, fly ash, quartz or silica ash, and the alkaline substance is sodium hydroxide.

[0017] Preferably, the silicon-aluminum raw material and the alkaline substance are mixed in a mass ratio of 1:(0.8-1.0), and then ground once to a particle size of less than 0.5 mm.

[0018] Preferably, the gelling active silica-alumina raw material is any one of metakaolin, fly ash, coal gasification slag, silica ash or a combination of several thereof.

[0019] Preferably, in step S22, the grinding to a particle size below 0.045 mm accounts for more than 75%.

[0020] The present invention further provides a geopolymer, wherein the geopolymer is prepared from the geopolymer dry powder material prepared according to the above-mentioned control method.

[0021] Finally, the present invention provides a method for preparing the geopolymer as described above, wherein the geopolymer dry powder material is used to prepare geopolymer slurry according to a water-cement ratio of 0.2 to 0.5, and the slurry is cured and dried to obtain the desired geopolymer.

[0022] Preferably, the curing is specifically as follows: the slurry is placed in a desired mold and shaken to expel bubbles, sealed and cured for 24 hours, then demoulded, and then placed in a humidity environment of 93% RH for further curing for at least 28 days.

[0023] The beneficial effects of the present invention are:

[0024] By adjusting the silicon-aluminum ratio and the alkali melting heat activation temperature of the silicon-aluminum raw materials, the physical phase of the calcined product can be adjusted. The calcined products with different physical phase structures release alkali in different forms and speeds after meeting water, and the reaction process of the calcined products with gelling active silicon-aluminum will also be different, thereby forming a method for regulating the reaction process of geopolymers.

[0025] Under the conditions of high silicon-aluminum ratio materials, the alkali-melt thermal activation product is mainly rich in sodium silicate phase. As the temperature increases, the reaction becomes more complete. When the temperature is low, the roasting product will exist in the form of a mixture of sodium silicate and sodium oxide. Under the conditions of medium and low silicon-aluminum ratio materials, the alkali-melt thermal activation product will contain sodium silicate and sodium aluminosilicate crystalline substances. As the silicon-aluminum ratio decreases and the temperature increases, the sodium aluminosilicate crystal content increases and the structure becomes more stable. It reacts weaker than sodium silicate when it comes into contact with water and has a slower dissolution rate. The later strength of the geopolymer can be controlled accordingly.

[0026] Therefore, under the action of different silicon-aluminum ratio raw materials and alkali melting heat activation temperature, the obtained calcined products can regularly regulate the properties of geopolymers.

[0027] For a certain geopolymer, the performance of the prepared geopolymer dry powder can be adjusted by adjusting the classification of the raw materials for its preparation and adaptively increasing or decreasing the raw material silicon-aluminum ratio and / or the roasting temperature according to this method. This method can greatly improve the applicability of geopolymers in the fields of construction engineering materials and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the preparation method of the present invention.

[0029] Figure 2 is the compressive strength of the sample prepared in Example 1.

[0030] Figure 3 This is the solidification time of the sample prepared in Example 1.

[0031] Figure 4 is the compressive strength of the sample prepared in Example 2.

[0032] Figure 5 is the compressive strength of the sample prepared in Example 3.

[0033] Figure 6 This is the compressive strength of the samples prepared in Examples 1-3 after 28 days of curing.

[0034] Figure 7 This is the compressive strength of the samples prepared in Examples 1-3 after 56 days of curing. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is described in more detail below in conjunction with the embodiments.

[0036] Example 1

[0037] The geopolymer preparation process includes the following steps:

[0038] S1. Quartz and alumina are mixed in a certain proportion to obtain silicon-aluminum raw materials with different silicon-aluminum ratios (1.5, 2, 6, 8, 12, 20);

[0039] S2. The silicon-aluminum raw material and sodium hydroxide were mixed and ground according to a mass ratio of 1.2, and then calcined at a low temperature (350° C.), and after calcination, the ore was ground to 0.074 mm to obtain low-temperature calcined materials with different silicon-aluminum ratios;

[0040] S3. Kaolin-rich coal gangue is converted into metakaolin by calcination at 700℃ for 8h, which is used as the raw material for gelling active silica-alumina;

[0041] S4. The low-temperature calcined material is mixed with the gelled active silica-alumina raw material, the mass of the low-temperature calcined material accounts for 15% of the total mass of the gelled active silica-alumina raw material and the low-temperature calcined material, and the silicon-aluminum ratio of the mixed material is 2.5. Then they are ground together until the particle size of all powders is below 0.045 mm to obtain the required geopolymer dry powder.

[0042] The prepared homogenized geopolymer dry powder was used to prepare geopolymer slurry according to a water-cement ratio of 0.33. After being fully stirred, the slurry was placed in a cubic mold with a side length of 100 mm. After being shaken to remove the bubbles in the slurry, it was sealed and cured at room temperature for 24 hours, and then demolded and placed in a curing box with a humidity of 93% for further curing.

[0043] like Figure 2The figure shows the compressive strength statistics of samples (prepared with low-temperature roasted materials) at different curing ages. It can be seen that the 3-day compressive strength of the geopolymer block gradually decreases with the action of high, medium and low silicon-aluminum ratio roasted materials, but the 7-, 28- and 56-day compressive strength of the geopolymer block first increases and then decreases with the action of high, medium and low silicon-aluminum ratio roasted materials. The early strength (3 days) of the geopolymer sample prepared with high silicon-aluminum ratio material is higher, but the later strength increases slowly. As the silicon-aluminum ratio of the material decreases, the strength of the sample increases significantly in the middle and late stages. However, when the aluminum-silicon ratio of the roasted material is too low (<6), the compressive strength of the sample decreases significantly. This is mainly due to the formation of a large amount of crystalline aluminosilicates in the roasted material, which restricts the release of active silicon and aluminum in the roasted material. In addition, as the silicon-aluminum ratio of the roasted material decreases, the solidification time of the sample gradually shortens, such as Figure 3 Therefore, when the calcination temperature is constant, the properties of geopolymer dry powder (such as compressive strength under long curing time) can be adjusted based on the adjustment of silicon-aluminum ratio.

[0044] Example 2

[0045] The geopolymer preparation process includes the following steps:

[0046] S1. Quartz and alumina are mixed in a certain proportion to obtain silicon-aluminum raw materials with different silicon-aluminum ratios (1.5, 2, 6, 8, 12, 20);

[0047] S2. The silicon aluminum raw material and sodium hydroxide were mixed and ground according to a mass ratio of 1.2, and then calcined at a medium temperature (500° C.), and after calcination, the ore was ground to 0.074 mm to obtain a high-temperature calcined material;

[0048] S3. Kaolin-rich coal gangue is converted into metakaolin by calcination at 700℃ for 8h, which is used as the raw material for gelling active silica-alumina;

[0049] S4. The medium temperature roasted material is mixed with the gelled active silica-alumina raw material, the mass of the medium temperature roasted material accounts for 15% of the total mass of the gelled active silica-alumina raw material and the medium temperature roasted material, and the silicon-aluminum ratio of the mixed material is 2.5. Then they are ground together until the particle size of all powders is below 0.045 mm to obtain the required geopolymer dry powder.

[0050] The prepared homogenized geopolymer dry powder was used to prepare geopolymer slurry according to a water-cement ratio of 0.33. After being fully stirred, the slurry was placed in a cubic mold with a side length of 100 mm. After being shaken to remove the bubbles in the slurry, it was sealed and cured at room temperature for 24 hours, and then demolded and placed in a curing box with a humidity of 93% for further curing.

[0051] like Figure 4The compressive strength statistics of the samples (prepared by medium-temperature roasted materials) at different curing ages show that within the same curing age, the compressive strength of the geopolymer prepared by roasting materials at 500°C is higher than that of the samples prepared by roasting materials at 350°C. The appropriate temperature increases the activity of the roasted materials, which is beneficial to the growth of the strength of the geopolymer.

[0052] Example 3

[0053] The geopolymer preparation process includes the following steps:

[0054] S1. Quartz and alumina are mixed in a certain proportion to obtain silicon-aluminum raw materials with different silicon-aluminum ratios (1.5, 2, 6, 8, 12, 20);

[0055] S2. The silica-alumina raw material is mixed with sodium hydroxide in a mass ratio of 1.2 and ground, and then roasted at a high temperature (700°C). After roasting, the ore is ground to 0.074 mm to obtain a high-temperature roasted material; S3. The kaolin-rich coal gangue is converted into metakaolin by calcining at 700°C for 8 hours, which is used as a gelling active silica-alumina raw material;

[0056] S4. The high-temperature calcined material is mixed with the gelled active silica-alumina raw material, the mass of the high-temperature calcined material accounts for 15% of the total mass of the active silica-alumina raw material and the medium-temperature calcined material, and the silicon-aluminum ratio of the mixed material is 2.5. Then they are ground together until the particle size of all powders is below 0.045 mm to obtain the required geopolymer dry powder.

[0057] The prepared homogenized geopolymer dry powder was used to prepare geopolymer slurry according to a water-cement ratio of 0.33. After being fully stirred, the slurry was placed in a cubic mold with a side length of 100 mm. After being shaken to remove the bubbles in the slurry, it was sealed and cured at room temperature for 24 hours, and then demolded and placed in a curing box with a humidity of 93% for further curing.

[0058] like Figure 5 From the statistical graph of compressive strength of samples (prepared with high-temperature calcined materials) at different curing ages, it can be seen that within the same curing age, the compressive strength of geopolymers prepared with materials calcined at 700°C is lower than that of samples prepared with materials calcined at 350°C and 500°C, but the change pattern is basically the same. This phenomenon can be attributed to the increase in calcination temperature, which leads to a decrease in the activity of the calcined materials, thereby restricting the growth rate of geopolymer strength.

[0059] The 28-day compressive strength data of the samples in Examples 1-3 are summarized as follows: Figure 6 The compressive strength data of the samples in Examples 1-3 on the 56th day are concentrated, and the results are shown in Figure 7. Since the 28th day, the strength of the prepared geopolymer meets the following requirements: 1) the compressive strength of the calcined materials prepared at the same temperature: medium silicon-aluminum ratio > high silicon-aluminum ratio > low silicon-aluminum ratio; 2) the compressive strength of the calcined materials prepared at the same silicon-aluminum ratio: medium temperature > low temperature > high temperature. Finally, the compressive strength of the geopolymers prepared by the 9 calcined materials decreased in the order of medium silicon-aluminum ratio-medium temperature materials, medium silicon-aluminum ratio-low temperature materials, medium silicon-aluminum ratio-high temperature materials, high silicon-aluminum ratio-medium temperature materials, high silicon-aluminum ratio-low temperature materials, high silicon-aluminum ratio-high temperature materials, low silicon-aluminum ratio-medium temperature materials, low silicon-aluminum ratio-low temperature materials, and low silicon-aluminum ratio-high temperature materials. That is, the enhancement of the compressive strength of the medium silicon-aluminum ratio-medium temperature materials is a positive condition, and the reduction of the compressive strength of the low silicon-aluminum ratio-high temperature materials is a positive condition. Therefore, for a certain geopolymer, by adjusting the classification of the raw materials used to prepare it, the performance of the prepared geopolymer dry powder can be adjusted by adaptively increasing or decreasing the silicon-aluminum ratio and / or calcination temperature of the raw materials according to this method.

[0060] The above implementation modes are only used to illustrate the technical solutions of the present invention, but not to limit the present invention. Although the present invention has been described in detail with reference to the above implementation modes, those skilled in the art should understand that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for controlling the performance of geopolymer dry powder materials, characterized in that: The following steps are involved: S1. Preparation of roasting materials S11. Confirm the classification of silicon-aluminum raw materials: the silicon-aluminum raw materials include high silicon-aluminum ratio, medium silicon-aluminum ratio, and low silicon-aluminum ratio. The silicon-aluminum ratio of the high silicon-aluminum ratio is greater than or equal to 15, the silicon-aluminum ratio of the medium silicon-aluminum ratio is 6-10, and the silicon-aluminum ratio of the low silicon-aluminum ratio is 1-6; S12. The silicon-aluminum raw material is mixed with an alkaline substance in a set ratio, and the mixed material is divided into three parts according to a set ratio, and high-temperature roasting, medium-temperature roasting, and low-temperature roasting are performed respectively, wherein the high-temperature roasting temperature is 600 to 700 ° C, the medium-temperature roasting temperature is 400 to 600 ° C, and the low-temperature roasting temperature is 250 to 400 ° C; Thus, 9 kinds of roasting materials are obtained, namely, high silicon-aluminum ratio-high temperature material, high silicon-aluminum ratio-medium temperature material, high silicon-aluminum ratio-low temperature material, medium silicon-aluminum ratio-high temperature material, medium silicon-aluminum ratio-medium temperature material, medium silicon-aluminum ratio-low temperature material, low silicon-aluminum ratio-high temperature material, low silicon-aluminum ratio-medium temperature material, and low silicon-aluminum ratio-low temperature material; S2. Preparation of geopolymers S21. According to the compressive strength of the geopolymer to be prepared, any 1 to 9 of the 9 calcined materials are selected and mixed to obtain a mixed calcined material; S22. The mixed roasted material and the gel active silica-alumina raw material are mixed in a mass ratio of (0.10-0.25):1 to obtain a mixed material, and the silica-alumina ratio of the gel active silica-alumina raw material is controlled so that the silica-alumina ratio of the mixed material is 2-5. The mixed material is ground to obtain the desired geopolymer dry powder material.

2. A method for controlling the performance of a geopolymer dry powder material according to claim 1, characterized in that: The mixing strategy of the nine kinds of roasting materials is: sorted by the weight of influence on compressive strength, in order: medium silicon-aluminum ratio-medium temperature material, medium silicon-aluminum ratio-low temperature material, medium silicon-aluminum ratio-high temperature material, high silicon-aluminum ratio-medium temperature material, high silicon-aluminum ratio-low temperature material, high silicon-aluminum ratio-high temperature material, low silicon-aluminum ratio-medium temperature material, low silicon-aluminum ratio-low temperature material, low silicon-aluminum ratio-high temperature material, and medium silicon-aluminum ratio-medium temperature material is a positive condition for enhancing the compressive strength, and low silicon-aluminum ratio-high temperature material is a positive condition for reducing the compressive strength, and as the silicon-aluminum ratio of the roasting material decreases, the solidification time of the slurry is shortened.

3. A method for controlling the performance of a geopolymer dry powder material according to claim 1, characterized in that: The silicon-aluminum raw material is one or more of coal gangue, fly ash, quartz or silica ash; and the alkaline substance is sodium hydroxide.

4. A method for controlling the performance of a geopolymer dry powder material as claimed in claim 3, characterized in that: The silicon-aluminum raw material and the alkaline substance are mixed in a mass ratio of 1: (0.8-1.0), and then ground once to a particle size of less than 0.5 mm.

5. A method for controlling the performance of a geopolymer dry powder material according to claim 1, characterized in that: The gelling active silica-alumina raw material is any one of metakaolin, fly ash, coal gasification slag and silica ash or a combination of several of them.

6. A method for controlling the performance of a geopolymer dry powder material according to claim 1, characterized in that: In the step S22, the powder is ground to a particle size below 0.045 mm, accounting for more than 75%.

7. A geopolymer, characterized in that The geopolymer dry powder material is prepared according to the control method according to any one of claims 1 to 6.

8. A method for preparing a geopolymer as claimed in claim 7, characterized in that: The geopolymer dry powder material is used to prepare geopolymer slurry according to a water-cement ratio of 0.2 to 0.5, and the slurry is cured and dried to obtain the required geopolymer.

9. The preparation method according to claim 8, characterized in that: The curing is specifically as follows: the slurry is placed in a desired mold and shaken to expel air bubbles, sealed and cured for 24 hours, then demolded, and then placed in a humidity environment of 93% RH and continued to be cured for at least 28 days.

Citation Information

Patent Citations

  • Method for preparing high-strength geopolymer cementing material from aluminum ash

    CN112341017A

  • Geopolymer dry powder material and preparation method thereof

    CN113003968A

  • Alkali-activated tailing-based composite cementing material and preparation method thereof

    CN113121132A

  • Method for predicting active silica-alumina ratio of alkali heat activated geopolymer raw material

    CN114113183A

  • Geopolymer compositions, cementitious composition comprising the same, and methods for making the same

    US20210087109A1

Cited By

  • Low-carbon cementing material and preparation method thereof

    CN119774899A

  • A low-carbon cementitious material and its preparation method

    CN119774899B