Preparation method of fly ash composite material
Through specific proportion mixing of fly ash, LLDPE and additives and hot pressing molding technology, composite materials with high density, high hardness and high flexural strength are prepared, which solves the problem of insufficient performance in the existing technology and is suitable for a variety of applications. field.
Patent Information
- Application Number
- CN202410868966.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technology cannot effectively prepare composite materials of fly ash and linear low-density polyethylene (LLDPE) with high density, high hardness, and high flexural strength.
Fly ash, LLDPE and talc powder are mixed according to the mass ratio of 23:9.3:1, and zinc oxide powder and sodium silicate powder are added after heating and melting. The composite material is prepared through hot pressing molding technology, using 316 stainless steel mesh as the skeleton. , control pressure and temperature to form high-performance composite materials.
The prepared fly ash composite material has high density, hardness and flexural strength, and is suitable for the manufacture of heat insulation, sound insulation materials and automobile parts, significantly improving the performance of the composite material.
Smart Images

Figure CN118771850A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fly ash composite materials, and in particular to a preparation method of a fly ash composite material. Background Art
[0002] Fly ash refers to a solid granular substance produced by burning a certain amount of coal when producing industrial raw materials such as cement, lime, and gypsum. The main components include aluminosilicates, aluminoferrites, and carbonates. These substances are solid particles with porous structures. It is precisely because of these porous structures that fly ash has many physical properties. For example, after high-temperature calcination, fly ash will form various substances, and will further form glass beads. The diameter of this glass bead is relatively small and has a very large specific surface area. This is because when fly ash is calcined, the aluminosilicate contained in it will react chemically with water and eventually form some gel particles. These gel particles will become glass beads after high-temperature calcination, which is the main use of fly ash in industrial production. After processing fly ash, a large number of functional products can be obtained. At present, fly ash has been widely used in chemical industry, construction and other fields. However, a large amount of harmful substances often remain after fly ash is processed. Therefore, the preparation of plastic composite materials using fly ash has become a very ideal treatment method.
[0003] Linear low-density polyethylene is a non-toxic, odorless milky white particle with a density of 0.916-0.934g / cm 3 , high strength, good toughness, high rigidity, heat resistance, impact resistance, tear resistance, and acid, alkali, organic solvent resistance, etc. As a multi-purpose thermoplastic material, it is widely used in various fields. Due to its excellent tensile strength and toughness, linear low-density polyethylene is widely used in the manufacture of various plastic bags and packaging films, such as shopping bags, garbage bags, bread bags, etc. In the agricultural field, it is used to make agricultural mulch, agricultural water pipes, etc. In the medical field, due to its lower melting temperature, it is suitable for medical devices and instruments that require low-temperature processing. Due to its wear resistance, aging resistance, softness, crystallinity and other characteristics, linear low-density polyethylene can increase the service life of wires and cables.
[0004] Based on the above background, in order to promote the resource utilization of industrial waste and promote the development of the field of composite materials, fly ash, as a common industrial waste, not only occupies land, but also may cause environmental pollution when it is piled up in large quantities. By compounding it with linear low-density polyethylene (LLDPE), a new composite material can be prepared, which can not only solve the problem of fly ash treatment, but also provide new material options for the field of composite materials. By optimizing the preparation process and composition ratio of composite materials, the performance of composite materials can be further improved to meet the needs of different fields. For example, in the field of construction, composite materials with high strength and high weather resistance can be prepared for construction; in the field of automobiles, composite materials for automobiles with lightweight and high impact resistance can be prepared. These optimized composite materials will play an important role in their respective fields and promote the development and progress of related industries.
[0005] However, up to now, there is no simple and efficient method to prepare a composite material of fly ash and LLDPE with high density, high hardness and high flexural strength.
[0006] Therefore, it is necessary to propose a method for preparing a fly ash composite material to solve the above problems. Summary of the invention
[0007] The present invention aims at the problem of how to simply and efficiently prepare a fly ash and LLDPE composite material with high density, high hardness and high flexural strength, and proposes a method for preparing a fly ash composite material, comprising the following steps:
[0008] S1. Mix fly ash, LLDPE and talcum powder in a mass ratio of 23:9.3:1 to obtain a main mixture;
[0009] S2, adding zinc oxide powder in a mass ratio of 1:1 to talcum powder to the main mixture, then heating and melting at one time, keeping the temperature for 45 minutes, and obtaining a premix when LLDPE reaches a molten state;
[0010] S3, then heating the premix a second time, adding sodium silicate powder in a mass ratio of 1:1 to talcum powder to the premix, keeping the temperature for 30 minutes, and stirring evenly to obtain a viscous mixture;
[0011] S4. Pour the melted mixture into a homemade mold while it is still hot. When the depth reaches half of the mold, put in a 316 stainless steel mesh as a skeleton. Then pour in the remaining half of the mixture. Flatten the upper surface of the mixture. Use hot pressing technology to keep the pressure on the composite material sheet at 10 MPa for 1 hour, then place it in a ventilated place to cool and shape. Finally, remove the mold and open it to obtain the fly ash composite material. Use a cutting machine to cut samples to test performance.
[0012] In a preferred embodiment of the present invention, the temperature of the primary heating and melting in S2 is 126°C.
[0013] In a preferred embodiment of the present invention, the temperature of the secondary heating in S3 is 200°C.
[0014] In a preferred embodiment of the present invention, the self-made mold in S4 is a box-shaped structure with dimensions of 10 cm×10 cm×(6.3-1.2) cm in length, width and height.
[0015] Furthermore, in S4, before using the mold, a layer of polytetrafluoroethylene plastic film is laid in the mold in advance, and after the mixture is poured into the mold and the upper surface is flattened, another layer of polytetrafluoroethylene plastic film is covered and hot pressing is performed.
[0016] Further, the area of the 316 stainless steel mesh is 90% of the upper surface area of the fly ash composite material in the mold, and the mass is 3-5% of the total mass of the fly ash composite material in the mold.
[0017] The fly ash composite material obtained by the preparation method of the fly ash composite material has a density of 1.4129 g / cm 2 , bending strength is 3.6MPa, hardness is 68 (HD), impact resistance is 1.998J / cm 2 Gangue composite materials can be used in the fields of thermal insulation, sound insulation, building materials and automobile parts manufacturing.
[0018] Implementing the embodiments of the present invention has the following beneficial effects:
[0019] The method for preparing the fly ash composite material of the present invention has a simple and efficient process. The prepared fly ash composite material has good high density, high hardness and high bending strength, and can be used in the fields of heat insulation, sound insulation materials, building materials and automobile parts manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 The schematic diagram is a process flow diagram of a method for preparing a fly ash composite material;
[0022] Figure 2 It is a structural diagram of the homemade mold;
[0023] Figure 3The SEM images of the fly ash composite materials prepared in Examples 1-3;
[0024] Figure 4 The DSC test result diagram of the fly ash composite material prepared in Examples 1-3;
[0025] Figure 5 TG curves of the fly ash composite materials prepared in Examples 1-3. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] See also Figure 1 , Figure 1 The figure is a schematic flow chart of a method for preparing a fly ash composite material; the method for preparing a fly ash composite material of the present invention comprises the following steps:
[0028] Step 1: Mix fly ash, LLDPE and talcum powder in a mass ratio of 23:9.3:1 to obtain a main mixture.
[0029] Step 2: Add zinc oxide powder in a mass ratio of 1:1 to talcum powder to the main mixture, and then heat and melt it at 126° C. for 45 minutes. When LLDPE reaches a molten state, a premix is obtained.
[0030] Step 3: Then heat the premix a second time at 200° C., add sodium silicate powder in a mass ratio of 1:1 to talcum powder into the premix, keep warm for 30 minutes, and stir evenly to obtain a viscous mixture.
[0031] Step 4: Before using the mold, lay a layer of polytetrafluoroethylene plastic film in the mold in advance, and pour the melted mixture into the homemade 10cm×10cm×(6.3-1.2)cm box-shaped mold while it is still hot. Figure 2 , Figure 2This is a structural diagram of the homemade mold. When the depth reaches half of the mold depth, a 316 stainless steel mesh is placed as a skeleton. The area of the 316 stainless steel mesh is 90% of the upper surface area of the fly ash composite material in the mold, and the mass is 3-5% of the total mass of the fly ash composite material in the mold. Then pour the remaining half of the mixture, flatten the upper surface of the mixture, and cover it with a layer of polytetrafluoroethylene plastic film. Use hot pressing technology to maintain a pressure of 10Mpa on the composite material sheet for 1 hour, then place it in a ventilated place to cool and shape, and finally remove the mold to open the mold to obtain the fly ash composite material, and use a cutting machine to cut samples to test performance.
[0032] The fly ash composite material obtained by the preparation method of the fly ash composite material has a density of 1.4129 g / cm 2 , bending strength is 3.6MPa, hardness is 68 (HD), impact resistance is 1.998J / cm 2 Gangue composite materials can be used in the fields of thermal insulation, sound insulation, building materials and automobile parts manufacturing.
[0033] Example 1
[0034] Preparation of 68% fly ash composite material:
[0035] The total amount of the main mixture used in the experiment is 150g, accurately weigh 102g of fly ash, LLDPE 40.5g, then add 7.5g of talcum powder, the mass ratio of the three raw materials is 13.6:5.4:1, add 7.5g of zinc oxide powder to the main mixture, then pour it into a blender and stir, then pour it into a beaker, use a glass rod to continue to mix the three evenly, use a constant temperature magnetic heating jacket to heat, use a program to increase the temperature, set it to 126°C, stay for 45min, and get a premix after LLDPE melts. Continue to heat and heat, keep it at about 200°C, add 7.5g of sodium silicate powder to the premix, continue to stir with a glass rod, keep warm for 30min, mix it thoroughly until it becomes viscous, and get a mixture. Transfer the mixture to a mold (60mm×60mm) covered with a polytetrafluoroethylene film, flatten it with a glass rod, cover it with a film, use hot pressing technology to keep the pressure on the composite material sheet at 10Mpa for 1h, then put it in a ventilated place to cool and shape, and finally remove the mold to open the mold. The size of the prepared plate is 60 mm×60 mm and the thickness is 12 mm. The prepared composite material plate is cut into samples using a cutting machine to test the performance.
[0036] Example 2
[0037] Preparation of 69% fly ash composite material:
[0038] The total amount of the main mixture used in the experiment is 150g, accurately weigh 103.5g of fly ash, LLDPE 39g, then add 7.5g of talcum powder, the mass ratio of the three raw materials is 13.8:5.2:1, add 7.5g of zinc oxide powder to the main mixture, then pour it into a blender and stir, then pour it into a beaker, continue to mix the three evenly with a glass rod, use a constant temperature magnetic heating jacket to heat, use a program to increase the temperature, set it to 126°C, stay for 45min, and get a premix after LLDPE melts. Continue to heat and heat, keep it at about 200°C, add 7.5g of sodium silicate powder to the premix, continue to stir with a glass rod, keep warm for 30min, mix it thoroughly until it becomes viscous, and get a mixture. Transfer the mixture to a mold (100mm×100mm) covered with a polytetrafluoroethylene film, flatten it with a glass rod, cover it with a film, use hot pressing technology to keep the pressure on the composite material sheet at 10Mpa for 1h, then put it in a ventilated place to cool and shape, and finally remove the mold to open the mold. The size of the prepared plate is 100 mm×100 mm and the thickness is 12 mm. The prepared composite material plate is cut into samples using a cutting machine to test the performance.
[0039] Example 3
[0040] Preparation of 69% fly ash composites with 316 stainless steel mesh added:
[0041] The total amount of the main mixture in the experiment is 150g. Accurately weigh 103.604g of fly ash and 41.892g of LLDPE. Then add 4.504g of zinc oxide powder. The mass ratio of the three raw materials is 23:9.3:1. Add 4.504g of zinc oxide powder to the main mixture, then pour it into a blender and stir, then pour it into a beaker, and continue to mix the three evenly with a glass rod. Use a constant temperature magnetic heating jacket to heat, use a program to increase the temperature, set it to 126℃, stay for 45min, and get a premix after LLDPE melts. Continue to heat and raise the temperature, maintain about 200℃, add 4.504g of sodium silicate powder to the premix, continue to stir with a glass rod, keep warm for 30min, mix thoroughly until it becomes viscous, and get a mixture. Then, lay a layer of polytetrafluoroethylene plastic in the mold before using it. The material film is poured immediately into a homemade 10cm×10cm×1.2cm box-shaped mold while the melted mixture is still hot. When the depth reaches half of the mold depth, a 316 stainless steel mesh is put in as a skeleton. The area of the 316 stainless steel mesh is 90% of the upper surface area of the fly ash composite material in the mold, and the mass is 3-5% of the total mass of the fly ash composite material in the mold. Then pour in the remaining half of the mixture, flatten the upper surface of the mixture, and then cover it with a layer of polytetrafluoroethylene plastic film. Use hot pressing technology to keep the pressure on the composite material sheet at 10Mpa for 1 hour, then place it in a ventilated place to cool and shape, and finally remove the mold to open the mold to obtain the fly ash composite material, and use a cutting machine to cut samples to test performance.
[0042] The fly ash composite materials of Examples 1-3 were characterized and tested for performance:
[0043] 1. SEM characterization:
[0044] Three test sample plates were collected and their bending sections were observed by scanning electron microscopy (SEM). A layer of conductive adhesive was applied on the test samples, and then after gold spraying, the surface morphology of the test samples was studied by SEM.
[0045] See also Figure 3 , Figure 3The SEM images of fly ash composite materials prepared in Example 1 (FA addition amount 68%), Example 2 (FA addition amount 69%), and Example 3 (FA addition amount 69% + stainless steel mesh); during the hot pressing process, the organic polymer resins are entangled with each other and wrapped in the cracks and surface of the fly ash. With the addition of fly ash, a large number of fly ash particles will appear at the interface of the cross section. When the composite material is bent, it will show a rigid side, making the composite material brittle. In addition, when more fly ash is added, the cracks between PE and fly ash become more obvious, indicating that there is no chemical reaction between the two, and when the amount of fly ash added increases, the compatibility between the two becomes very poor, and it is difficult to achieve uniform mixing. Therefore, how to fully mix the two and form a stable and continuous interface on their surface is a key problem to be solved in this research field.
[0046] 2.DSC characterization:
[0047] The melting point, crystallization temperature and melting enthalpy of the composite material were determined by DSC thermal analysis. In a nitrogen atmosphere, the material was heated to 200°C at 20°C / min, cooled to 40°C at 20°C / min after 2 minutes, and then heated to 200°C at a heating rate of 20°C / min, and the enthalpy changes during the melt and crystallization process were recorded.
[0048] The test results are as follows Figure 4 As shown, the corresponding DSC data are listed in Table 1:
[0049] Table 1 Parameters of melt crystallization properties of three composite materials
[0050]
[0051] Depend on Figure 4 As shown in Table 1, the amount of fly ash added has little effect on the melting peak temperature of the composite material, and its melting point ranges from 118°C to 123°C. At the same time, with the addition of fly ash, the crystallization peak temperature of the composite material also changes, indicating that after the addition of fly ash, the crystallization temperature of the composite material undergoes heterogeneous nucleation. In addition, it can be seen from the melting curve that the greater the amount of fly ash added, the smaller the melting point width, the smaller the melting peak area, and the lower the melting enthalpy.
[0052] According to the melting enthalpy data of the DSC curve, the crystallinity of the composite material can be calculated using the formula. The crystallinity of the composite material is shown in Table 1:
[0053]
[0054] Where, X C —Crystallinity of composite materials, %;
[0055] ΔHm—melting crystallization enthalpy of the sample, J / g;
[0056] ΔHm 0 — Melting enthalpy of complete crystallization of PE, 289 J / g;
[0057] w—mass fraction of PE in the composite material, %;
[0058] Please refer to Table 2, which shows the crystallinity results of the three composite materials:
[0059] Table 2 Crystallinity of different composite materials
[0060]
[0061]
[0062] As shown in Table 2, the addition of fly ash changes the crystallinity of the composite material, indicating that it plays an important role as a crystal nucleating agent in the composite material.
[0063] 3. TGA characterization:
[0064] The sample was divided into several parts, and thermal analysis was performed on each of them, and the thermal weight loss during heating was measured. The test conditions were set as follows: reaction atmosphere air, heating rate 20℃ / min, temperature range 40-1000℃.
[0065] Test results such as Figure 5 As shown, the corresponding TG data are listed in Table 3:
[0066] Table 3 TG data of composite materials prepared with different fly ash addition amounts
[0067]
[0068] Depend on Figure 5 From the data analysis of Table 3, it can be seen that with the addition of fly ash, the pyrolysis temperature of the composite material gradually increases. When the amount of fly ash added reaches 5%, the pyrolysis temperature of the composite material reaches 342.52℃, 291.08℃, and 349.98℃. At the same time, with the addition of fly ash, the maximum decomposition temperature of the composite material also increases. At 600℃, with the increase of fly ash dosage, the mass retention rate of the composite material gradually increases. This phenomenon may be due to the thermal decomposition of PE at 200℃, which makes it have good thermal stability, and the addition of fly ash will hinder its thermal conductivity, thereby improving its thermal stability. In addition, since a large amount of fly ash is added during the decomposition of PE at 600℃, the mass retention rate of the composite material is also improved.
[0069] 4. Performance test:
[0070] The mass of the composite material (prepared in Example 1) was measured by an analytical balance to be 75.3989 g, and the volume was measured by the displacement method to be 58.9 cm 3 , by the formula ρ=m / v, the density ρ of the composite material is calculated to be 0.7058g / cm 3 . The hardness of the sample was measured to be 52 (HD) using the LX-D Shore hardness tester produced by Taizhou AiCe Instrument Co., Ltd. The bending strength of the sample was measured to be 0.73MPa using the WDW-20 microcomputer-controlled electronic universal testing machine produced by Changchun Xinte Testing Machine Co., Ltd. The impact resistance was tested using a simply supported beam impact testing machine produced by Chengde Kebiao Testing Instrument Manufacturing Co., Ltd. The result was 0.492J / cm 2 .
[0071] The mass of the composite material (prepared in Example 2) was measured by an analytical balance to be 130.8840 g, and the volume was measured by the displacement method to be 100 cm 3 , the density of the composite material is calculated to be 1.3088 g / cm by the formula ρ = m / v. 3 . The hardness of the sample was measured to be 48 (HD) using the LX-D Shore hardness tester produced by Taizhou AiCe Instrument Co., Ltd. The bending strength of the sample was measured to be 0.61MPa using the WDW-20 microcomputer-controlled electronic universal testing machine produced by Changchun Xinte Testing Machine Co., Ltd. The impact resistance was tested using a simply supported beam impact testing machine produced by Chengde Kebiao Testing Instrument Manufacturing Co., Ltd. The result was 0.403J / cm 2 .
[0072] The mass of the composite material (prepared in Example 3) was measured by an analytical balance to be 138.1807 g, and the volume was measured by the displacement method to be 97.8 cm 3 , by the formula ρ=m / v, the density ρ of the composite material is calculated to be 1.4129g / cm 3 . The hardness of the sample was measured to be 68 (HD) using the LX-D Shore hardness tester produced by Taizhou AiCe Instrument Co., Ltd. The bending strength of the sample was measured to be 3.6MPa using the WDW-20 microcomputer-controlled electronic universal testing machine produced by Changchun Xinte Testing Machine Co., Ltd. The impact resistance was tested using a simply supported beam impact testing machine produced by Chengde Kebiao Testing Instrument Manufacturing Co., Ltd. The result was 1.998J / cm 2 .
[0073] 5. Analysis of the influence of different dosages on composite materials:
[0074] The present invention selects a total experimental dosage of 150g, a pressure of 10MPa, and a hot pressing time of 1 hour, and uses hot pressing molding technology to prepare a composite material, and studies the density, hardness, thickness, bending strength and other performance parameters of the composite material when the fly ash content is 68%, 69%, and 69% with stainless steel mesh. It can be seen from the experimental results that when 150g of fly ash is added in the experiment, the fly ash content increases from 68% to 69%, which increases the density of the composite material by 85.43% and the hardness by 7.69%. The study found that with the increase in the amount of fly ash, the density, hardness and other properties of the composite material drop sharply. The research and analysis results show that the fly ash (69% content)-LLDPE composite material prepared by adding stainless steel mesh is the best ratio, with a bending strength of 3.6MPa and a density of 1.4129g / cm 3 .
[0075] The present invention is of great significance for promoting the resource utilization of industrial waste and promoting the development of the composite material field. Fly ash is a common industrial waste. Large amounts of accumulation not only occupy land, but also may cause environmental pollution. By compounding it with linear low-density polyethylene (LLDPE) and adding talcum powder, zinc oxide powder and sodium silicate powder, a new composite material is prepared, which can not only solve the problem of fly ash treatment, but also provide new material options for the composite material field. By optimizing the preparation process, composition ratio and the like of the composite material, the performance of the composite material can be further improved to meet the needs of different fields. For example, in the field of construction, a composite material for construction with high strength and high weather resistance can be prepared; in the field of automobiles, a composite material for automobiles with lightweight and high impact resistance can be prepared. These optimized composite materials will play an important role in their respective fields and promote the development and progress of related industries.
[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a fly ash composite material, characterized in that: The following steps are involved: S1. Mix fly ash, LLDPE and talcum powder in a mass ratio of 23:9.3:1 to obtain a main mixture; S2, adding zinc oxide powder in a mass ratio of 1:1 to talcum powder to the main mixture, then heating and melting at one time, keeping the temperature for 45 minutes, and obtaining a premix when LLDPE reaches a molten state; S3, then heating the premix a second time, adding sodium silicate powder in a mass ratio of 1:1 to talcum powder to the premix, keeping the temperature for 30 minutes, and stirring evenly to obtain a viscous mixture; S4. Pour the melted mixture into a homemade mold while it is still hot. When the depth reaches half of the mold, put in a 316 stainless steel mesh as a skeleton. Then pour in the remaining half of the mixture. Flatten the upper surface of the mixture. Use hot pressing technology to keep the pressure on the composite material sheet at 10 MPa for 1 hour, then place it in a ventilated place to cool and shape. Finally, remove the mold and open it to obtain the fly ash composite material. Use a cutting machine to cut samples to test performance.
2. The method for preparing the fly ash composite material according to claim 1, characterized in that: The temperature of the first heating and melting in S2 is 126°C.
3. The method for preparing the fly ash composite material according to claim 1, characterized in that: The temperature of the secondary heating in S3 is 200°C.
4. The method for preparing the fly ash composite material according to claim 1, characterized in that: The homemade mold in S4 is a box-shaped structure with dimensions of 10 cm×10 cm×(6.3-1.2) cm in length, width and height.
5. The method for preparing the fly ash composite material according to claim 4, characterized in that: In the above-mentioned S4, a layer of polytetrafluoroethylene plastic film is laid in the mold before using the mold. After the mixture is poured into the mold and the upper surface is flattened, another layer of polytetrafluoroethylene plastic film is laid on the mold for hot pressing.
6. The method for preparing the fly ash composite material according to claim 5, characterized in that: The area of the 316 stainless steel mesh is 90% of the upper surface area of the fly ash composite material in the mold, and the mass is 3-5% of the total mass of the fly ash composite material in the mold.
7. The method for preparing the fly ash composite material according to any one of claims 1 to 6, characterized in that: The fly ash composite material obtained by the preparation method of the fly ash composite material has a density of 1.4129 g / cm 2 , bending strength is 3.6MPa, hardness is 68HD, impact resistance is 1.998J / cm 2 .
8. The method for preparing the fly ash composite material according to claim 7, characterized in that: The coal gangue composite material is used in the fields of heat insulation, sound insulation, building materials and automobile parts manufacturing.
Citation Information
Patent Citations
Fly ash-enhanced polymer composite material interlocking type ground tile and preparation method thereof
CN101768907A
Method for preparing composite board by filling LLDPE with high-content CFB fly ash
CN114571648A