Preparation methods of high-entropy rare-earth silicate ceramic powders and bulks and ceramic powders
By developing a method for preparing high-entropy rare-earth silicate ceramic powder, the corrosion problem of ceramic materials in high-temperature water vapor environments has been solved, achieving high density and uniformity of the material, improving its resistance to water vapor and stability, and expanding its application areas.
Patent Information
- Application Number
- CN202410818441.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-24
AI Technical Summary
In existing technologies, ceramic materials are prone to corrosion in high-temperature and water-gas environments, leading to unstable product quality, insufficient resistance to water vapor, and inaccurate temperature control and silica addition, which affect material performance and stability.
A high-entropy rare-earth silicate ceramic powder preparation method was adopted. The molar ratio of rare-earth oxides to silicon dioxide was controlled by solid-state pressureless sintering, and hot-pressing sintering was carried out under argon protection. The heat treatment and sintering parameters were optimized to ensure the uniformity and density of the material.
It significantly improves the high-temperature water vapor corrosion resistance of ceramic materials, maintains a stable structure in high-temperature environments, reduces production costs, and broadens the application range.
Smart Images

Figure CN118771887B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-performance ceramic technology, and particularly relates to a method for preparing high-entropy rare earth silicate ceramic powder and bulk with high temperature and water vapor corrosion resistance, as well as the ceramic powder. Background Technology
[0002] Ceramic matrix composites are increasingly being used in aircraft components to protect the matrix from high-temperature water vapor corrosion, resulting in the preparation of water vapor corrosion resistant materials.
[0003] Prior art document 1 (CN202111526882.1) discloses a low thermal conductivity high entropy ceramic thermal barrier coating material, prior art document 2 (CN202311262101.1) discloses a high entropy rare earth silicate ceramic powder resistant to high temperature water and oxygen corrosion and its preparation method, and prior art document 3 (CN201911196312.3) discloses a γ-type high entropy rare earth disilicate with ultra-high temperature stability and its preparation method.
[0004] The main technical problems existing in the technology include:
[0005] 1. Insufficient temperature accuracy: Inaccurate temperature measurement or control equipment can lead to inaccurate temperature control during production, affecting the composition and properties of materials. This can result in unstable product quality or products that do not meet requirements.
[0006] 2. Inaccurate addition of silica: As an additive in materials, inaccurate addition of silica leads to deviations in the material composition, affecting the material's performance and stability. This can result in products failing to meet performance standards in areas such as high-temperature resistance and water / oxygen corrosion.
[0007] 3. Insufficient resistance to moisture: The material's insufficient resistance to moisture causes the product to be corroded by moisture during use, which in turn affects its service life and performance stability.
[0008] To address the above problems and shortcomings, it is necessary to further improve existing technologies, enhance the accuracy of temperature control, ensure precise control of additives, and improve the water vapor resistance of materials, thereby improving product quality and performance. Summary of the Invention
[0009] To address the problems existing in the prior art, this invention provides a method for preparing high-entropy rare earth silicate ceramic powder and bulk with high-temperature water vapor corrosion resistance, aiming to solve the problem that the high impurity content of high-entropy rare earth disilicates in the prior art affects their resistance to water oxygen corrosion.
[0010] This invention is achieved by providing a method for preparing high-entropy rare-earth silicate ceramic powder and bulk with high-temperature water vapor corrosion resistance, comprising the following steps:
[0011] Step 1: Mix Re2O3 powder and silica powder to obtain a mixed powder;
[0012] Step 2: Mix the powder and ethanol solution to obtain a slurry; mix using a ball mill for 12-24 hours, dry, and pass through a 100-mesh sieve to obtain powder 1;
[0013] Step 3: After heat treatment, remove and grind using a ball mill and anhydrous ethanol. Dry and pass through a 200-sieve to obtain powder 2;
[0014] Step 4: Powder 2 is loaded into a graphite mold and pre-room temperature cold pressing is performed using a powder tablet press. Then, hot pressing sintering is performed in a hot press furnace with a protective atmosphere to obtain high-entropy rare earth silicate ceramic powder and bulk with high temperature water vapor corrosion resistance.
[0015] The Re2O3 powder includes Yb2O3 powder, Y2O3 powder, Lu2O3 powder, Er2O3 powder, and Sc2O3 powder. The molar ratio of Yb2O3, Y2O3, Lu2O3, Er2O3, and Sc2O3 is 1:1:1:1:1. The molar ratio of Re2O3 to SiO2 is 1:1.15. The molar ratio of silicon to rare earth elements is 1 to 1.3:1.
[0016] Furthermore, in step three, the heat treatment temperature is 1350–1520℃, the heat treatment time is 2–5h, and the heating rate is 2–8℃ / min.
[0017] Furthermore, the protective atmosphere described in step four is argon.
[0018] Furthermore, in step four, the pressure applied during cold pressing is 10–17 MPa.
[0019] Furthermore, in step four, the heating rate for hot pressing sintering is 5–10 °C / min, the sintering temperature is 1200 °C–1520 °C, the sintering time is 3–10 hours, and the sintering pressure is 20–40 MPa.
[0020] Another objective of this invention is to provide a high-entropy rare earth silicate ceramic powder and a high-entropy rare earth silicate ceramic powder with high-temperature water vapor corrosion resistance prepared by a method for preparing such powder and the powder having the molecular formula (Re)2Si2O7, wherein Re is composed of a molar ratio of Yb, Y, Er, Lu, and Sc.
[0021] Furthermore, the particle size of the ceramic powder is 10–75 μm.
[0022] Based on the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solution to be protected by this invention are as follows:
[0023] First, to address the problem of high impurity content in existing high-entropy rare-earth silicates affecting their resistance to water and oxygen corrosion, this invention provides high-entropy rare-earth silicate ceramic powder resistant to high-temperature water and oxygen corrosion and its preparation method. The high-entropy rare-earth silicate powder of this invention is prepared by solid-state pressureless sintering. The high-entropy rare-earth silicate material prepared by this invention can form a stable single-phase solid solution, with uniform element distribution, high purity, simple operation, and low cost. Furthermore, this system of high-entropy rare-earth silicates exhibits excellent resistance to water and oxygen corrosion; after corrosion for 200 hours in a quasi-static water and oxygen environment at 1400℃ and 50% H2O-50% O2, the weight loss rate is only 0.001-0.01%.
[0024] In this invention, the secondary phase is a monosilicate, and the impurity is SiO2; the weight loss rate after 200 h is 0.01%.
[0025] This invention improves purity. This invention enhances resistance to moisture and air.
[0026] Second, the following describes the prior art problems solved by this invention and the significant technical advancements achieved:
[0027] In the field of materials science, especially in high-temperature environments, the performance of ceramic materials has always been a research hotspot. However, traditional ceramic materials often suffer severe corrosion in high-temperature water vapor environments, which limits their application in key fields such as aerospace and energy. This invention addresses this problem by proposing a method for preparing high-entropy rare-earth silicate ceramic powders and bulk materials with high-temperature water vapor corrosion resistance, bringing a new breakthrough to the field of materials science.
[0028] This invention successfully prepared high-entropy rare-earth silicate ceramics with excellent resistance to high-temperature water vapor corrosion by precisely controlling the molar ratio of raw materials and the preparation process. This material not only maintains a stable structure at high temperatures but also effectively resists water vapor corrosion, thus significantly improving the material's reliability and durability. This technological breakthrough provides a new solution for material applications in high-temperature environments.
[0029] Compared with traditional ceramic materials, the high-entropy rare-earth silicate ceramics of this invention have achieved significant progress in both preparation process and performance. Firstly, through solid-state pressureless sintering, this invention achieves low-temperature preparation of ceramic materials, reducing energy consumption and production costs. Secondly, by optimizing the raw material ratio and preparation process, this invention successfully improves the high-temperature water vapor corrosion resistance of the ceramic materials, giving them better stability and reliability in high-temperature environments. These technological advancements not only enhance the material's performance but also broaden its application range in various fields.
[0030] This invention, through innovative preparation methods and material design, successfully solves the problem of easy corrosion of traditional ceramic materials in high-temperature water vapor environments, achieving significant technological progress. This high-entropy rare-earth silicate ceramic material not only possesses excellent resistance to high-temperature water vapor corrosion but also boasts a simple and low-cost preparation process, demonstrating significant application value and market potential. In the future, with further technological development and optimization, it is believed that this material will demonstrate its unique advantages and potential in more fields.
[0031] Third, this invention provides a method for preparing high-entropy rare-earth silicate ceramic powder and bulk with high-temperature water vapor corrosion resistance, comprising the following steps: First, Yb2O3, Y2O3, Lu2O3, Er2O3 and Sc2O3 powders are mixed in a molar ratio of 1:1:1:1:1, and then mixed with silica powder in a molar ratio of 1:1.15 to obtain a mixed powder; then, the mixed powder is mixed with an ethanol solution, and the mixture is ball-milled for 12-24 hours, dried, and passed through a 100-mesh sieve to obtain... Powder 1; Next, powder 1 is heat-treated at 1350-1520℃ for 2-5 hours in air atmosphere, then ground with anhydrous ethanol for 4-8 hours, dried and passed through a 200-mesh sieve to obtain powder 2; Finally, powder 2 is loaded into a graphite mold, cold-pressed at 10-17MPa using a powder tablet press, and then hot-pressed and sintered at 1200℃-1520℃ in a hot press furnace with an argon protective atmosphere for 3-10 hours at a sintering pressure of 20-40MPa to obtain the final product.
[0032] This invention solves the problem of rare earth silicate ceramics being easily corroded by moisture in high-temperature environments. Traditional ceramic materials are prone to chemical reactions in high-temperature and humid environments, leading to a decline in material performance. By employing a high-entropy rare earth silicate system, this invention significantly improves the water vapor corrosion resistance of ceramic materials, enabling them to maintain a stable structure and excellent performance even under harsh high-temperature environments.
[0033] This invention introduces the concept of high-entropy alloys in the preparation process, improving the structural complexity and thermodynamic stability of the material through equimolar mixing of various rare earth oxides. This high-entropy effect not only enhances the corrosion resistance of the ceramic but also strengthens its thermal shock resistance and mechanical strength. Simultaneously, by optimizing heat treatment and sintering process parameters, such as controlling the heat treatment temperature between 1350 and 1520°C, the sintering temperature between 1200°C and 1520°C, and performing hot-pressing sintering under an argon protective atmosphere, the density and homogeneity of the material are ensured.
[0034] The significant technological advancements achieved by this invention are reflected in the following aspects: First, by introducing high-entropy alloying with multiple rare earth elements, the corrosion resistance and thermal shock resistance of ceramic materials are improved, enabling them to exhibit excellent stability in extreme environments; second, by precisely controlling heat treatment and sintering parameters, high density and uniformity of the material are achieved, further improving its mechanical properties and service life; finally, the method of this invention simplifies the process flow and reduces production costs, making the industrial application of high-performance rare earth silicate ceramics possible.
[0035] Fourth, this invention successfully prepared high-entropy rare-earth silicate ceramic powders and bulk materials resistant to high-temperature water vapor corrosion by precisely controlling the molar ratio of rare-earth oxides to silicon dioxide and employing specific heat treatment temperatures and times. This method overcomes the shortcomings of traditional ceramic materials that are easily corroded in water vapor environments, significantly improving the durability and stability of ceramics.
[0036] During the preparation process, ball milling is used for prolonged mixing to ensure uniform powder distribution. Specific heat treatment steps further optimize the material's microstructure and properties. This meticulous process control results in a final product with excellent resistance to high temperatures and water vapor corrosion, making it suitable for various extreme environments.
[0037] Furthermore, this invention uses argon as a protective atmosphere, effectively preventing material oxidation during hot-pressing sintering and ensuring product purity and performance. By adjusting the sintering heating rate, temperature, time, and pressure, high density and uniformity of the ceramic material are achieved, further enhancing its mechanical strength and corrosion resistance.
[0038] In summary, this invention significantly improves the high-temperature resistance and water vapor corrosion resistance of rare earth silicate ceramics through innovative material formulation and precise process control, providing strong technical support for the application of ceramic materials in extreme environments and representing an important technological advancement in this field. Attached Figure Description
[0039] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the embodiments of the present invention will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0040] Figure 1 This is a flowchart of the preparation method of high-entropy rare earth silicate ceramic powder and bulk with high temperature water vapor corrosion resistance provided by the embodiments of the present invention;
[0041] Figure 2 This is a successfully synthesized XRD pattern provided in an embodiment of the present invention;
[0042] Figure 3 These are the synthesis XRD patterns at different sintering temperatures provided in the embodiments of the present invention;
[0043] Figure 4 These are XRD patterns of different silica ratios synthesized according to embodiments of the present invention;
[0044] Figure 5 These are XRD comparison diagrams and phase ratio diagrams under different water vapor corrosion times provided in the embodiments of the present invention; (a)(Yb) 0.2 Y 0.2 Lu 0.2 Er 0.2 Sc 0.2 )2Si2O7;
[0045] (b)(Yb 0.25 Y 0.25 Lu 0.25 Er 0.25 )2Si2O7(c)Yb2Si2O7;
[0046] Figure 6 This is a percentage diagram of different phases provided in an embodiment of the present invention;
[0047] Figure 7 This is a weightlessness rate diagram provided in an embodiment of the present invention; Detailed Implementation
[0048] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0049] like Figure 1 As shown in the figure, the present invention provides a method for preparing high-entropy rare-earth silicate ceramic powder and bulk with high-temperature water vapor corrosion resistance, comprising the following steps:
[0050] Step 1: Weigh out Yb2O3 powder, Y2O3 powder, Lu2O3 powder, Er2O3 powder, Sc2O3 powder and SiO2 in a molar ratio of 1:1:1:1:1.15. Use zirconia balls as the mixing medium. The solid-liquid ratio of powder to anhydrous ethanol is 1:1.5 and the ball-to-material ratio is 5:1.
[0051] Step 2: Dissolve rare earth silicate powder and silicon dioxide powder completely in anhydrous ethanol to obtain a solution, so that the molar ratio of silicon to rare earth elements is 1.15:1; the resulting slurry is first ball-milled for 12-24 hours at a speed of 500 r / min, and then the ball-milled slurry is placed in an 80℃ oven for 12 hours to dry, and then filtered through a 100-mesh sieve to obtain powder 1;
[0052] Step 3: Powder 1 is sintered for 120 minutes in muffle furnaces at 1350℃, 1400℃, 1450℃, 1480℃, and 1520℃ respectively, with 1480℃ being the optimal preparation temperature and a heating rate of 5℃ / min. The sintered powder is then placed in a ball mill jar with a solid-liquid ratio of 1:1.5 for powder and anhydrous ethanol, using zirconia balls as the mixing medium at a ball-to-powder ratio of 5:1. The powder is then ball-milled for 8-12 hours at a speed of 500 r / min, and then dried in an 80℃ oven. Finally, powder 2 is obtained by passing the powder through a 200-mesh sieve.
[0053] Step 4: Weigh about 1.2g of the dried powder 2 that has passed through a 200-mesh sieve and put it into a cylindrical mold with a diameter of 12mm. Use a powder tablet press to form tablet 1 at room temperature under a pressure of 15MPa. Then, use a hot press furnace to perform hot pressing treatment on tablet 1, sintering at 1480℃ for 300min at a pressure of 30MPa and a heating rate of 5℃ / min to obtain a dense tablet 2.
[0054] The high-entropy rare earth silicate ceramic powder resistant to high-temperature water and oxygen corrosion provided in this embodiment of the invention has the molecular formula (RE)2Si2O7, wherein RE is a combination of Yb, Y, Er, Lu and Sc; the high-entropy rare earth silicate powder of this invention is prepared by solid-state pressureless sintering, and the particle size of the ceramic powder is 10-75 μm.
[0055] This invention provides a method for preparing high-entropy rare-earth silicate ceramic powder and bulk with high-temperature water vapor corrosion resistance. The specific steps are as follows:
[0056] Step 1: Raw material preparation and mixing
[0057] Weigh out Yb2O3 powder, Y2O3 powder, Lu2O3 powder, Er2O3 powder, Sc2O3 powder and SiO2 in a molar ratio of 1:1:1:1:1.15.
[0058] Zirconia balls are used as a mixing medium to ensure uniform powder mixing.
[0059] The solid-liquid ratio of the powder to anhydrous ethanol is controlled at 1:1.5, and the ball-to-particle ratio is 5:1.
[0060] Step 2: Dissolving and ball milling
[0061] The rare earth silicate powder and silicon dioxide powder were completely dissolved in anhydrous ethanol to ensure that the molar ratio of silicon to rare earth elements was 1.15:1.
[0062] The resulting slurry was ball-milled for 12-24 hours at a speed of 500 r / min to achieve a more uniform mixing effect.
[0063] The ball-milled slurry was dried in an 80℃ oven for 12 hours, and then filtered through a 100-mesh sieve to obtain powder 1.
[0064] Step 3: Sintering and re-ball milling
[0065] Powder 1 was subjected to a first sintering of 120 min in a muffle furnace at different temperatures (1350℃, 1400℃, 1450℃, 1480℃, and 1520℃), with 1480℃ being the optimal preparation temperature.
[0066] The heating rate was set to 5℃ / min to ensure the stability of the sintering process.
[0067] The sintered powder was placed back into a ball mill jar, and anhydrous ethanol and zirconia balls were added for ball milling for 8-12 hours at the same speed of 500 r / min.
[0068] The ball-milled powder was dried again in an 80°C oven and finally passed through a 200-mesh sieve to obtain powder 2.
[0069] Step 4: Tableting and hot pressing sintering
[0070] Weigh approximately 1.2g of the dried powder 2 that has passed through a 200-mesh sieve and place it into a cylindrical mold with a diameter of 12mm.
[0071] Tablet 1 is formed by cold pressing at room temperature under a pressure of 15 MPa using a powder tablet press.
[0072] The tablet 1 is then subjected to hot pressing in a hot press furnace, sintered at 1480℃ for 300 min at a pressure of 30 MPa and a heating rate of 5℃ / min, to obtain a dense tablet 2.
[0073] The high-entropy rare-earth silicate ceramic powder of this invention has the molecular formula (RE)₂Si₂O₇, where RE is a combination of Yb, Y, Er, Lu, and Sc. This ceramic powder is prepared by solid-state pressureless sintering and has a particle size of 10–75 μm. Due to its unique composition and preparation method, this high-entropy rare-earth silicate ceramic material exhibits excellent resistance to high-temperature water vapor corrosion and has broad application prospects in high-temperature environments such as aerospace and energy.
[0074] Two specific application examples are as follows:
[0075] 1. In the aerospace field, this high-entropy rare-earth silicate ceramic material can be used as a protective coating for hot-end components of engines, effectively resisting high-temperature water vapor corrosion and improving the reliability and durability of engines.
[0076] 2. In the energy sector, especially in nuclear power generation, this material can serve as a thermal insulation layer or protective material inside the reactor. While withstanding high-temperature water vapor corrosion, it also possesses good thermal and radiation stability, ensuring the safe operation of the nuclear reactor.
[0077] The embodiments of the present invention have achieved some positive results during the research and development or use process, and have indeed great advantages compared with the prior art. The following content describes them in conjunction with the data, charts and other information of the experimental process.
[0078]
[0079]
[0080] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications, equivalent substitutions, and improvements made by those skilled in the art within the scope of the technology disclosed in the present invention, and within the spirit and principles of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a high-entropy rare earth silicate ceramic powder with high temperature water vapor corrosion resistance, characterized in that, Includes the following steps: Step 1: Mix Re2O3 powder and silica powder to obtain a mixed powder; Step 2: Mix the powder and ethanol solution to obtain a slurry; mix using a ball mill for 12-24 hours, dry, and pass through a 100-mesh sieve to obtain powder 1; Step 3: Powder 1 is heat-treated in air atmosphere, anhydrous ethanol is added, it is ground for 4-8 hours, dried and passed through 200 sieves to obtain high-entropy rare earth silicate ceramic powder with high temperature water vapor corrosion resistance. The Re2O3 powder includes Yb2O3 powder, Y2O3 powder, Lu2O3 powder, Er2O3 powder, and Sc2O3 powder. The molar ratio of Yb2O3, Y2O3, Lu2O3, Er2O3, and Sc2O3 is 1:1:1:1:1, and the molar ratio of silicon to rare earth elements is 1.15:
1. In step three, the heat treatment temperature is 1350–1520℃, the heat treatment time is 2–5h, and the heating rate is 2–8℃ / min.
2. A high-entropy rare-earth silicate ceramic powder resistant to high-temperature water-oxygen corrosion prepared by the preparation method as described in claim 1, characterized in that, The molecular formula is (Re)2Si2O7, where Re is a combination of Yb, Y, Er, Lu and Sc in molar ratio.
3. The high-entropy rare-earth silicate ceramic powder as described in claim 2, characterized in that, The ceramic powder has a particle size of 10–75 μm.
4. A method for preparing a high-entropy rare-earth silicate ceramic bulk with resistance to high-temperature water vapor corrosion, characterized in that, The process includes the following steps: preparing high-entropy rare-earth silicate ceramic powder according to the method described in claim 1; loading the ceramic powder into a graphite mold, performing pre-room temperature cold pressing molding using a powder press, and hot pressing sintering in a hot press furnace with a protective atmosphere to obtain the high-entropy rare-earth silicate ceramic block.
5. The method for preparing the high-entropy rare-earth silicate ceramic bulk with high-temperature water vapor corrosion resistance as described in claim 4, characterized in that, The protective atmosphere is argon.
6. The method for preparing the high-entropy rare-earth silicate ceramic bulk with high-temperature water vapor corrosion resistance as described in claim 4, characterized in that, The pressure applied during cold pressing is 10–17 MPa.
7. The method for preparing the high-entropy rare-earth silicate ceramic bulk with high-temperature water vapor corrosion resistance as described in claim 4, characterized in that, The heating rate for hot pressing sintering is 5-10℃ / min, the sintering temperature is 1200℃-1520℃, the sintering time is 3-10 hours, and the sintering pressure is 20-40MPa.
Citation Information
Patent Citations
γ-type high-entropy rare earth disilicates with ultra-high temperature stability and their preparation method
CN111056826B
A low thermal conductivity, high entropy ceramic thermal barrier coating material
CN114149260B
High-entropy rare earth silicate ceramic powder resistant to high-temperature water and oxygen corrosion and preparation method thereof
CN117362035A
Gamma-type high-entropy rare earth disilicate with ultrahigh-temperature stability and preparation method thereof
CN111056826A
CMAS-corrosion-resistant high-entropy ceramic material with small grain size and preparation method of CMAS-corrosion-resistant high-entropy ceramic material
CN114671675A