A method for preparing mesophase carbon microsphere-based porous carbon material

By mixing asphalt with nanoceramic fibers and silicone oil for emulsification polymerization and high-temperature carbonization, combined with pickling treatment, an intermediate phase carbon microsphere-based porous carbon material with excellent electrochemical properties was prepared, which solved the corrosion resistance of the equipment in the prior art. The problems of high performance, uneven pore structure and low energy density have achieved the preparation of porous carbon materials with high specific surface area and regular pore structure.

CN118790979BActive Publication Date: 2024-11-26KEDA (ANHUI) NEW MATERIAL CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411278076.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-26
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

During the preparation of existing intermediate phase carbon microsphere porous carbon materials, there are problems such as high corrosion resistance, uneven pore structure and low energy density in the equipment, which are difficult to mass production on a large scale and difficult to regulate the pore structure.

Method used

The asphalt was mixed with nanoceramic fibers and silicone oil and then sonicated, followed by emulsification polymerization, preoxidation and high-temperature carbonization, combined with pickling treatment to prepare an intermediate phase carbon microsphere-based porous carbon material with uniform distribution of nanoceramic fibers.

Benefits of technology

A porous carbon material with high compaction density, high particle strength, large specific surface area and regular pore structure is achieved, showing excellent electrochemical performance and rate performance, with specific surface area ≥2250m2/g, and specific capacitance at 1 A/g current density ≥300F/g, the retention rate is ≥80% at 10A/g current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118790979B_ABST
    Figure CN118790979B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a mesophase carbon microsphere-based porous carbon material, which belongs to the technical field of lithium ion battery and supercapacitor electrode materials, and comprises the following steps: (1) crushing raw asphalt; (2) mixing the crushed asphalt with nano-ceramic fibers and silicone oil in a certain mass ratio and ultrasonicating to obtain a mixed solution; (3) pouring the mixed solution into a reactor, stirring and heating, and then cooling to room temperature; (4) centrifuging the emulsion and washing the solid product with petroleum ether and anhydrous ethanol for multiple centrifugal washings, and then drying; (5) placing the solid product in a rotary kiln, heating and then keeping the temperature to obtain pre-oxidized asphalt microspheres; (6) placing the pre-oxidized asphalt microspheres in a high-temperature carbonization furnace; (7) pickling the mesophase carbon microspheres and acid in a certain mass ratio, washing to neutrality after pickling, and drying to obtain a precursor material; and (8) placing the precursor material in a high-temperature carbonization furnace for high-temperature carbonization to obtain the mesophase carbon microsphere-based porous carbon material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery and supercapacitor electrode materials, and in particular to a method for preparing a mesophase carbon microsphere-based porous carbon material. Background Art

[0002] Porous carbon materials have abundant micropores and mesopores and high specific surface area, and play an important role in various fields as adsorbents, catalytic carriers and energy storage materials. Such a wide range of applications is mainly attributed to the large pore range and special pore characteristics (such as specific surface area, pore size distribution and pore volume) of porous carbon.

[0003] Mesocarbon microbeads (MCMB) are micron-sized spherical carbon materials with a nematic liquid crystal layered stacking structure generated by thermal polycondensation of heavy aromatic compounds such as asphalt. MCMB has been widely studied due to its advantages such as excellent electrical conductivity and mechanical stability. Due to the high orientation of the MCMB carbon layer, it is easy to occupy the open pores formed by the overflow of volatiles during the carbonization process. At present, alkali activation is used to prepare porous carbon from MCMB materials. Patent CN114835115A pre-treats the mesocarbon microbeads, performs intercalation and capacity expansion, and allows the alkali activator to penetrate into the interior of the mesocarbon microbeads for activation reaction. The specific surface area of ​​the prepared mesocarbon microbeads reaches 3371.3m 2 / g, the specific capacitance reaches 840F / g. However, the preparation process involves the use of alkaline materials, which requires high corrosion resistance of the equipment and cannot be mass-produced. In addition, the uniformity of the pore structure of the prepared porous carbon material is difficult to effectively control. The compaction density of the material is reduced by intercalation expansion, thereby reducing the energy density of the material. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing mesophase carbon microsphere-based porous carbon material, which overcomes the defects and shortcomings of the above-mentioned prior art.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a mesophase carbon microsphere-based porous carbon material comprises the following steps:

[0007] (1) Crushing the raw asphalt;

[0008] (2) mixing the crushed asphalt in step (1) with nano-ceramic fibers and silicone oil in a certain mass ratio and ultrasonically treating the mixture to obtain a mixed liquid;

[0009] (3) pouring the mixed solution in step (2) into a reaction kettle, under an inert atmosphere, controlling the stirring rate at 100-300 r / min, heating to 400-500°C and keeping the temperature for 4-8 hours, then naturally cooling to room temperature and taking out the emulsion in the kettle;

[0010] (4) centrifuging the emulsion obtained in step (3) and washing the solid product by centrifugation multiple times with petroleum ether and anhydrous ethanol, and finally drying the solid product in a vacuum oven to obtain mesophase asphalt microspheres;

[0011] (5) placing the solid product in step (4) in a rotary kiln, heating it to 200-350° C. in an oxidizing atmosphere, and keeping it at that temperature for 2-6 hours to obtain pre-oxidized asphalt microspheres;

[0012] (6) placing the pre-oxidized asphalt microspheres prepared in step (5) in a high-temperature carbonization furnace, heating the furnace to 800-900° C. under an inert atmosphere, and keeping the temperature for 1-3 h to obtain mesophase carbon microspheres;

[0013] (7) acid-washing the mesophase carbon microspheres prepared in step (6) with acid in a certain mass ratio, washing with deionized water until neutral, and finally drying to obtain a precursor material;

[0014] (8) Placing the precursor material prepared in step (7) in a high-temperature carbonization furnace, heating it to 1200-1400° C. in an inert atmosphere, and keeping the temperature for 1-3 h to obtain a mesophase carbon microsphere-based porous carbon material.

[0015] The present invention further defines the technical solution:

[0016] Furthermore, the mass ratio of the crushed asphalt to the nano-ceramic fiber and the silicone oil in (2) is 1: (1-2): (10-20), and the ultrasonic time after mixing is at least 1 hour.

[0017] Furthermore, the nano-ceramic fiber is one of silicon dioxide nano-fiber, zirconium oxide nano-fiber and aluminum oxide nano-fiber, and has a diameter of 10-50 nm and a length of 20-30 um.

[0018] Furthermore, the oxidizing atmosphere is a mixed gas of one or more of oxygen and air, and the inert atmosphere is a mixed gas of one or two of nitrogen and argon.

[0019] Furthermore, in said (7), the mesophase carbon microspheres prepared in step (6) are pickled with acid in a mass ratio of 1:(2-5), the pickling temperature is 20-70°C, the pickling time is 0.5-5h, after pickling, deionized water is used to wash to neutrality, and finally dried at 80°C-120°C for 6-10h to obtain a precursor material.

[0020] Furthermore, the acid used in pickling is at least one of dilute sulfuric acid, dilute nitric acid, dilute hydrochloric acid, dilute acetic acid and hydrofluoric acid, and the acid concentration is 1-5 mol / L.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention adds asphalt powder and nano-ceramic fibers to silicone oil and then ultrasonically stirs them evenly, then places them in a reactor for emulsification polymerization to form mesophase asphalt microspheres with nano-ceramic fibers evenly distributed inside, then prepares mesophase carbon microspheres with nano-ceramic fibers evenly distributed inside through pre-oxidation and carbonization treatment, and finally prepares spherical porous carbon materials with high compaction density, high particle strength, large specific surface area, evenly distributed pore structure and relatively regular pore structure through acid washing and high-temperature carbonization. The overall pore structure has low tortuosity, provides a rapid diffusion channel for the transmission of ions, and exhibits excellent electrochemical properties.

[0023] The present invention overcomes the shortcomings of the prior art preparation method, such as low specific surface area and uneven pore structure, and the prepared porous carbon material has a specific surface area of ​​≥2250m 2 / g, the specific capacitance is ≥300F / g at a current density of 1 A / g, and the specific capacitance retention rate is ≥80% at a current density of 10A / g, showing excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart for preparing the mesophase carbon microsphere-based porous carbon material of the present invention;

[0025] Figure 2 This is a SEM image of the mesocarbon microsphere-based porous carbon material prepared in Example 1;

[0026] Figure 3 This is the nitrogen adsorption-desorption curve of the mesocarbon microsphere-based porous carbon material prepared in Example 1;

[0027] Figure 4 This is the pore size distribution diagram of the mesophase carbon microsphere-based porous carbon material prepared in Example 1. DETAILED DESCRIPTION

[0028] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with embodiments. It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.

[0029] Example 1

[0030] This embodiment provides a method for preparing a mesocarbon microsphere-based porous carbon material, which specifically includes the following steps:

[0031] (1) The raw asphalt is crushed and sieved through a 300-mesh sieve;

[0032] (2) Mixing the crushed asphalt in step (1) with nano-ceramic fibers and silicone oil in a mass ratio of 1:1.5:15 and ultrasonicating for 1 hour to ensure that the three are fully mixed and uniformly prepared to obtain a mixed solution;

[0033] (3) Pour the mixed solution in step (2) into a reaction kettle, control the stirring rate at 200 r / min under an inert atmosphere, raise the temperature to 450°C and keep it for 6 hours, then cool it naturally to room temperature and take out the emulsion in the kettle;

[0034] (4) centrifuging the emulsion obtained in step (3) and washing the solid product by centrifugation multiple times with petroleum ether and anhydrous ethanol, and finally drying the solid product in a vacuum oven to obtain mesophase asphalt microspheres;

[0035] (5) placing the solid product in step (4) in a rotary kiln, heating it to 300° C. in an oxidizing atmosphere, and keeping it at that temperature for 4 h to obtain pre-oxidized asphalt microspheres;

[0036] (6) placing the pre-oxidized asphalt microspheres prepared in step (5) in a high-temperature carbonization furnace, heating to 850° C. under an inert atmosphere, and keeping the temperature for 2 h to obtain mesophase carbon microspheres;

[0037] (7) pickling the mesophase carbon microspheres prepared in step (6) with acid in a mass ratio of 1:3 at a temperature of 40° C. for 2 h, washing with deionized water until neutral, and finally drying at 90° C. for 8 h to obtain a precursor material;

[0038] (8) The precursor material prepared in step (7) is placed in a high-temperature carbonization furnace, heated to 1300°C under an inert atmosphere, and kept at this temperature for 2 hours to obtain a mesophase carbon microsphere-based porous carbon material having a surface morphology as shown in FIG. Figure 2 As shown, the porous carbon has a good spherical morphology, uniform size, and an average particle size of 20.2 um.

[0039] The prepared mesophase carbon microsphere-based porous carbon material was subjected to nitrogen adsorption and desorption tests. The test curve is as follows: Figure 3 As shown, it exhibits a typical type I isotherm, and the material exhibits obvious gas adsorption in the area with relatively low gas pressure, indicating that the prepared porous carbon material is mainly filled with micropores.

[0040] Figure 4 This is the pore size distribution diagram of the mesophase carbon microsphere-based porous carbon material prepared in Example 1. It can be seen from the figure that the prepared porous carbon material is mainly composed of micropores. The pore volume of the micropores is 1.06 cm 3 / g, accounting for 86.88% of the total pore volume.

[0041] Comparative Example 1

[0042] Step a, uniformly mixing mesophase carbon microspheres and potassium hydroxide in a mass ratio of 1:2;

[0043] Step b, placing the uniformly mixed materials in step a in a tube furnace, and activating them at 800° C. for 2 h under an inert atmosphere to obtain a precursor material;

[0044] Step c: Mix the precursor material prepared in step b with 4M dilute hydrochloric acid at a mass ratio of 1:1, stir for 2 hours, filter, and wash with deionized water several times until neutral to obtain a porous carbon material.

[0045] Comparative Example 2

[0046] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, and the difference between it and Example 1 is that the mass ratio of the crushed asphalt and the nano-ceramic fiber is 1:0.5.

[0047] Comparative Example 3

[0048] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the mass ratio of the crushed asphalt to the nano-ceramic fiber is 1:2.5.

[0049] Comparative Example 4

[0050] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the diameter of the nano-ceramic fiber is 8 nm.

[0051] Comparative Example 5

[0052] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the diameter of the nano-ceramic fiber is 60 nm.

[0053] Comparative Example 6

[0054] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the stirring rate in step (3) is 80 r / min.

[0055] Comparative Example 7

[0056] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the pre-oxidation temperature in step (5) is 400°C.

[0057] Comparative Example 8

[0058] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the mass ratio of the mesophase carbon microspheres to the acid in step (7) is 1:1.

[0059] Comparative Example 9

[0060] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the high-temperature carbonization temperature in step (8) is 1000°C.

[0061] Comparative Example 10

[0062] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is basically the same as that in Example 1, except that the high-temperature carbonization temperature in step (8) is 1600°C.

[0063] Comparative Example 11

[0064] The preparation method of a mesophase carbon microsphere-based porous carbon material in this comparative example is the same as the steps in Example 1, and the difference between it and Example 1 is that nano-ceramic fibers are not added.

[0065] The preparation methods of mesophase carbon microsphere-based porous carbon materials provided in Examples 2-6 are basically the same as the method steps of Example 1, and the main differences are that the component ratios and process parameter settings are different, as shown in Table 1, and the high-temperature carbonization temperature in Table 1 refers to the temperature parameter involved in step (8) in the example.

[0066] The specific capacitance of porous carbon materials was tested by cyclic voltammetry, including preparing an electrode sheet with mesophase carbon microsphere-based porous carbon material, polytetrafluoroethylene (PTFE) and SP conductive carbon in a mass ratio of 8:1:1 as a working electrode, a platinum electrode as a counter electrode, and a Hg / HgO electrode as a reference electrode in a 6M KOH solution.

[0067] The test results of the physicochemical properties and electrical properties of the mesocarbon microsphere-based porous carbon materials prepared in the above-mentioned embodiments and comparative examples are shown in Tables 2 and 3.

[0068] Table 1 Ratios of components and process parameters in Examples 2-6

[0069]

[0070] Table 2 Physical and chemical properties of mesophase carbon microsphere-based porous carbon prepared in various embodiments of the present invention

[0071]

[0072] Table 3 Electrochemical performance parameters of mesophase carbon microsphere-based porous carbon prepared in various embodiments of the present invention

[0073]

[0074] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention shall be implemented according to the conventional means in the art unless otherwise specified and limited.

Claims

1. A method for preparing a mesophase carbon microsphere-based porous carbon material, characterized in that: The specific steps include: (1) Crushing the raw asphalt; (2) mixing the crushed asphalt in step (1) with nano-ceramic fibers and silicone oil in a certain mass ratio and ultrasonically treating the mixture to obtain a mixed liquid; (3) pouring the mixed solution in step (2) into a reaction kettle, under an inert atmosphere, controlling the stirring rate at 100-300 r / min, heating to 400-500°C and keeping the temperature for 4-8 hours, then naturally cooling to room temperature and taking out the emulsion in the kettle; (4) centrifuging the emulsion obtained in step (3) and washing the solid product by centrifugation multiple times with petroleum ether and anhydrous ethanol, and finally drying the solid product in a vacuum oven to obtain mesophase asphalt microspheres; (5) placing the solid product in step (4) in a rotary kiln, heating it to 200-350° C. in an oxidizing atmosphere, and keeping it at that temperature for 2-6 hours to obtain pre-oxidized asphalt microspheres; (6) placing the pre-oxidized asphalt microspheres prepared in step (5) in a high-temperature carbonization furnace, heating the furnace to 800-900° C. under an inert atmosphere, and keeping the temperature for 1-3 h to obtain mesophase carbon microspheres; (7) acid-washing the mesophase carbon microspheres prepared in step (6) with acid in a certain mass ratio, washing with deionized water until neutral, and finally drying to obtain a precursor material; (8) Placing the precursor material prepared in step (7) in a high-temperature carbonization furnace, heating it to 1200-1400° C. in an inert atmosphere, and keeping the temperature for 1-3 h to obtain a mesophase carbon microsphere-based porous carbon material.

2. The method for preparing a mesocarbon microsphere-based porous carbon material according to claim 1, characterized in that: The mass ratio of the crushed asphalt to the nano-ceramic fiber and the silicone oil in (2) is 1: (1-2): (10-20), and the ultrasonic time after mixing is at least 1 hour.

3. The method for preparing a mesocarbon microsphere-based porous carbon material according to claim 2, characterized in that: The nano ceramic fiber is one of silicon dioxide nano fiber, zirconium oxide nano fiber and aluminum oxide nano fiber, and has a diameter of 10-50 nm and a length of 20-30 um.

4. The method for preparing a mesocarbon microsphere-based porous carbon material according to claim 1, characterized in that: The oxidizing atmosphere is one or more mixed gases of oxygen and air, and the inert atmosphere is one or two mixed gases of nitrogen and argon.

5. The method for preparing a mesocarbon microsphere-based porous carbon material according to claim 1, characterized in that: In the step (7), the mesophase carbon microspheres prepared in step (6) are pickled with acid in a mass ratio of 1:(2-5), the pickling temperature is 20-70°C, the pickling time is 0.5-5h, after pickling, deionized water is used to wash until neutral, and finally, the precursor material is dried at 80°C-120°C for 6-10h to obtain the precursor material.

6. The method for preparing a mesocarbon microsphere-based porous carbon material according to claim 5, characterized in that: The acid used in pickling is at least one of dilute sulfuric acid, dilute nitric acid, dilute hydrochloric acid, dilute acetic acid and hydrofluoric acid, and the acid concentration is 1-5 mol / L.

Citation Information

Cited By

  • Preparation method of carbon microsphere-silicon negative electrode material

    CN120389030A