Aluminum-based composite current collector, preparation method thereof and application of aluminum-based composite current collector in negative-electrode-free sodium battery

By depositing a nanoflower-like zinc modification layer on the aluminum-based current collector, the problems of sodium dendrites growth and volume expansion in the negative electrode-free sodium batteries are solved, the Coulomb efficiency and cycle life of the battery are improved, and the stable solid electrolyte membrane is formed, which is improved. Overall performance of the battery.

CN119050372APending Publication Date: 2024-11-29ZHENGZHOU UNIV
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411177205.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the negative-node sodium battery, the low binding energy with sodium metal, the growth of sodium dendrite and the unstable interface of solid electrolytes, the battery banking efficiency and poor cycle life are caused, and the volume changes of metal sodium cannot be effectively regulated. Impacts the safety and electrochemical performance of the battery.

Method used

Using aluminum-based composite liquid collectors, nanoflower-like zinc modification layer is deposited through electroless plating technology to form a highly ordered porous structure, promote electrolyte penetration and ion transport, and regulate the uniform distribution and nucleation of sodium ions through the sodium-philic Zn layer. , inhibit dendrites' growth and volume expansion.

Benefits of technology

It achieves high Coulomb efficiency and excellent cycle life, forming a uniform, thin and inorganic solid electrolyte membrane, improving the stability and electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050372A_ABST
    Figure CN119050372A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of negative-electrode-free sodium battery current collector manufacturing, discloses an aluminum-based composite current collector, a preparation method thereof and application of the aluminum-based composite current collector in a negative-electrode-free sodium battery, and aims to solve the technical problem that the cycle life of the battery is short due to SEI (solid electrolyte interface) film breakage caused by sodium ion disordered deposition, sodium dendrite growth and volume expansion under high surface capacity. According to the aluminum-based composite current collector, nanoflowers with the diameter of 100-500 nm are assembled by nanosheets with the thickness of 1-5 nm, the thickness of a nanoflower-shaped zinc modification layer is 0.5-5 microns, and the aluminum-based composite current collector is prepared by depositing a nanoflower-shaped zinc layer on the surface of an aluminum foil in situ through a chemical plating process. The highly ordered porous structure in the aluminum-based composite current collector promotes the permeation of electrolyte and the transfer of ions; the highly-exposed crystal face edge has high catalytic activity on electrolyte reductive decomposition, and formation of stable SEI is facilitated; the sodium-philic zinc layer effectively promotes uniform distribution of sodium ions on the current collector and inhibits dendritic crystal growth buffer volume expansion. When the composite material is applied to a negative-electrode-free sodium metal battery, high coulombic efficiency and excellent cycle life of the battery can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of manufacturing current collectors for negative electrode-free sodium batteries, and in particular to an aluminum-based composite current collector and a preparation method thereof, and application thereof in negative electrode-free sodium batteries. Background Art

[0002] Rechargeable sodium batteries (RSBs) are an attractive option for “beyond lithium” electrochemical storage technology due to their high resource abundance and good economic / environmental sustainability. Most sodium batteries are sodium-ion batteries, which can provide cell-level specific energy of about 120-160 Wh / kg and can serve as an alternative to graphite LiFePO4 batteries for large-scale stationary storage. Currently, RSBs are expected to gain significant advantages over other competitors (higher energy density) and further expand their applications to electric vehicles and consumer electronics. Anode-free RSBs, which pair a thin and light aluminum current collector (as anode) with a high-voltage stable cathode, are expected to achieve a 17-35% increase in cell energy from deintercalable sodium-ion batteries and become an attractive candidate for batteries exceeding 300 Wh / kg.

[0003] However, the use of traditional aluminum foil and copper foil as current collectors has low binding energy with sodium metal, which leads to problems such as low battery coulombic efficiency, sodium metal dendrite growth and instability of solid electrolyte interface (SEI). In addition, traditional current collectors cannot alleviate the volume change of metallic sodium during battery cycling, resulting in changes in the internal structure of the battery, affecting the safety and electrochemical performance of the battery, which limits the practical application of anode-free sodium metal batteries. Therefore, developing high-performance current collectors for efficient uniform and dense deposition of sodium is one of the key technologies for developing high-energy-density anode-free sodium batteries.

[0004] The prior art discloses some sodium metal batteries with few negative electrodes or no negative electrode. For example, the patent application number CN118198376A discloses a modified current collector and its preparation and application in a metal battery without negative electrode. The patent uses conductive carbon black to coat the surface of the current collector, and then magnetron sputters a sodium-philic metal M surface layer (at least one of Ag, Au, Pb, Ga, and Zn) in the middle of the carbon particles to synthesize the modified current collector. However, due to the inability to control the structure of the metal M particles, it is impossible to stably cycle under high surface capacity conditions. The patent application number CN114373982A discloses a secondary sodium battery with few negative electrodes based on a liquid ether organic electrolyte and a preparation method thereof. Although the patent proposes that a modified material that can react with sodium ions and induce metal sodium deposition can be loaded on the surface of the current collector to improve the reversibility of half-cell electroplating stripping and the cycle life of the full battery, the improvement effect is not significant, resulting in poor cycle life and stability of the sodium battery without negative electrode. Therefore, how to regulate the current collector composite structure to further improve the cycle stability of high surface capacity negative electrode-free sodium batteries has become an urgent problem to be solved. Summary of the invention

[0005] In order to solve the problems of disordered deposition of sodium ions and growth of sodium dendrites under high surface capacity, volume expansion leading to rupture of SEI film, and poor battery cycle life under actual working conditions, the present invention proposes an aluminum-based composite current collector, a preparation method thereof, and application in a negative electrode-free sodium battery.

[0006] To achieve the above object, the technical solution of the present invention is implemented as follows: An aluminum-based composite current collector comprises an aluminum foil and a nano-flower-shaped zinc modification layer, wherein the nano-flower-shaped zinc modification layer is composed of nano-sheets with a thickness of 1-5 nm and nano-flowers with a diameter of 100-500 nm, and the thickness of the nano-flower-shaped zinc modification layer is 0.5-5 μm.

[0007] The preparation method of the above-mentioned aluminum-based composite current collector comprises the following steps: (1) Pre-treating the aluminum foil; (2) Deposition of a nano-flower-like zinc modification layer by chemical plating: Sodium hydroxide and zinc oxide are dissolved in deionized water to prepare a zinc plating solution, and then the aluminum foil pretreated in step (1) is immersed in the zinc plating solution and washed with deionized water. The immersion-washing process is repeated 2-5 times, and then dried to obtain an aluminum-based composite current collector.

[0008] The pretreatment in the above step (1) includes acetone treatment and H2SO4 solution treatment.

[0009] The above-mentioned acetone treatment refers to acetone ultrasonic cleaning for 10-60 s to remove oily impurities; the H2SO4 solution treatment refers to 0.1-1.5 M sulfuric acid treatment for 5-20 s to remove oxidized impurities on the surface of the aluminum foil.

[0010] In the above step (2), the concentration of sodium hydroxide in the zinc plating solution is 1-10 mol / L, and the concentration of zinc oxide is 0.02-0.3 mol / L.

[0011] The time of immersion in the zinc plating solution in the above step (2) is 5-30 s.

[0012] Application of the above-mentioned aluminum-based composite current collector in negative electrode-free sodium batteries.

[0013] A negative electrode-free sodium battery comprises a positive electrode sheet, an electrolyte, a diaphragm and the above-mentioned aluminum-based composite current collector or the aluminum-based composite current collector prepared by the above-mentioned preparation method.

[0014] The above-mentioned negative electrode-free sodium battery can be in the form of a button or a soft pack.

[0015] Furthermore, the positive electrode sheet comprises a positive electrode active material, a conductive agent and a binder; and the electrolyte comprises a sodium salt and an organic solvent.

[0016] Further, specifically, the above-mentioned positive electrode active material is any one of sodium vanadium phosphate, sodium iron pyrophosphate, sodium iron pyrophosphate and sodium manganese iron pyrophosphate; the conductive agent is any one or more of graphene, carbon nanotubes, acetylene black, Ketjen black or Super PLi; the binder is polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); the sodium salt is any one or more of sodium hexafluorophosphate, sodium perchlorate, sodium trifluoromethylsulfonate, sodium tetrafluoroborate, sodium bis(fluorosulfonyl)imide and sodium bis(trifluoromethylsulfonyl)imide; the organic solvent is any one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, diethylene glycol dimethyl ether, 1,3-cyclopentanediol, ethylene glycol dimethyl ether and triethylene glycol dimethyl ether; the diaphragm is any one of polyethylene, polypropylene microporous membrane, glass fiber membrane and polyacrylonitrile diaphragm.

[0017] The preparation method of the above-mentioned negative electrode-free sodium battery comprises the following steps: (1) The positive electrode active material, binder, and conductive agent were dissolved in N-methylpyrrolidone solvent at a mass ratio of 7:2:1 and stirred evenly to prepare a slurry. The slurry was applied on the current collector and dried overnight at 120°C in vacuum. Then, a 12 mm pole piece was punched and the pole piece loading was 32 mg cm -2 Making a positive electrode sheet; (2) Punch the aluminum-based composite current collector into a pole piece (16 mm in diameter), separate the pole piece from the positive electrode piece with a separator, and drip an electrolyte (1 M in concentration). Use a stainless steel shell as the outer shell to assemble into a CR2025 button battery.

[0018] The beneficial effects produced by the present invention are: (1) The present invention synthesizes a composite current collector for a negative electrode-free sodium metal battery with a highly ordered nanosheet cross-linked zinc layer on the current collector by a simple chemical plating process. The preparation process does not involve multiple coatings and is therefore simple, highly homogenized, environmentally friendly and safe, and can be industrially applied.

[0019] (2) The present invention designs a novel nanoflower-shaped zinc-modified aluminum-based composite current collector (Zn@Al) for a new type of negative electrode-free sodium battery. The highly ordered porous structure promotes the penetration of electrolyte and the transport of ions. At the same time, the highly exposed crystal surface edges have high catalytic activity for the reduction and decomposition of the electrolyte, promote electron transfer and accelerate the breaking of CF bonds or PF bonds in anions and the decomposition of solvents, forming a uniform, thin and inorganic SEI. At the same time, the sodium-philic Zn layer effectively promotes the uniform distribution of sodium ions on the current collector, regulates the uniform nucleation and subsequent stable growth of sodium metal, and inhibits dendrite growth and buffers volume expansion. When the aluminum-based composite current collector is applied to a negative electrode-free sodium battery, high coulombic efficiency and excellent cycle life are achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is an optical picture of Zn@Al-20 prepared in Example 1 of the present invention.

[0022] Figure 2 This is the X-ray diffraction (XRD) pattern of Zn@Al-20 prepared in Example 1 of the present invention.

[0023] Figure 3 This is a scanning electron microscope (SEM) image of Zn@Al-20 prepared in Example 1 of the present invention.

[0024] Figure 4 This is a scanning electron microscope-energy dispersive spectrometer (SEM-EDS) image of the cross section of Zn@Al-20 prepared in Example 1 of the present invention.

[0025] Figure 5 This is a Kelvin atomic force microscope (KPFM) image of Zn@Al-20 prepared in Example 1 of the present invention.

[0026] Figure 6 The half-cell assembled with the composite current collector of the negative electrode-free sodium metal battery prepared in Examples 1-6 of the present invention is -2 The current density and 1 mAh cm -2 Reversibility testing of electroplating and stripping under conditions of sodium deposition.

[0027] Figure 7 A high-resolution scanning electron microscope (HR-TEM) image of the Zn@Al-20 interface and a Fourier transform image corresponding to the lattice fringes of the SEI inorganic component after half-cell cycling of the Zn@Al-20 assembled according to Example 1 of the present invention.

[0028] Figure 8 The half-cell assembled with the composite current collector of the negative electrode-free sodium metal battery prepared in Example 1 of the present invention is 3 mAcm -2 The current density and 3 mAh cm -2 Reversibility testing of electroplating and stripping under conditions of sodium deposition.

[0029] Fig. 9 The symmetrical battery assembled with the composite current collector of the negative electrode-free sodium metal battery prepared in Example 1 of the present invention has a high conductivity at 1, 2, and 3 mA cm -2The current density and 1, 2, and 3 mAh cm -2 Dendrite suppression and cycle life tests.

[0030] Fig.10 The cycle performance curve (a) and charge-discharge curve (b) of a negative electrode-free sodium battery assembled with the aluminum-based composite current collector prepared in Example 1 are shown.

[0031] Fig.11 The cycle performance curve (a) and charge and discharge curve (b) of the negative electrode-free sodium battery assembled in Comparative Example 1.

[0032] Fig.12 The cycle performance curve (a) and charge-discharge curve (b) of the negative electrode-free sodium battery assembled with the current collector prepared in Comparative Example 2. DETAILED DESCRIPTION

[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0035] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0036] An aluminum-based composite current collector comprises an aluminum foil and a nano-flower-shaped zinc modification layer, wherein the nano-flower-shaped zinc modification layer is composed of nano-sheets with a thickness of 1-5 nm and nano-flowers with a diameter of 100-500 nm, and the thickness of the nano-flower-shaped zinc modification layer is 0.5-5 μm.

[0037] The preparation method of the above-mentioned aluminum-based composite current collector comprises the following steps: (1) Pre-treating the aluminum foil; (2) Deposition of a nano-flower-like zinc modification layer by chemical plating: Sodium hydroxide and zinc oxide are dissolved in deionized water to prepare a zinc plating solution, and then the aluminum foil pretreated in step (1) is immersed in the zinc plating solution and washed with deionized water. The immersion-washing process is repeated 2-5 times, and then dried to obtain an aluminum-based composite current collector.

[0038] The pretreatment in the above step (1) includes acetone treatment and H2SO4 solution treatment.

[0039] The above-mentioned acetone treatment refers to acetone ultrasonic cleaning for 10-60 s to remove oily impurities; the H2SO4 solution treatment refers to 0.1-1.5 M sulfuric acid treatment for 5-20 min to remove oxidized impurities on the surface of the aluminum foil.

[0040] In the above step (2), the concentration of sodium hydroxide in the zinc plating solution is 1-10 mol / L, and the concentration of zinc oxide is 0.02-0.3 mol / L.

[0041] The time of immersion in the zinc plating solution in the above step (2) is 5-30 s.

[0042] Application of the above-mentioned aluminum-based composite current collector in negative electrode-free sodium batteries.

[0043] A negative electrode-free sodium battery comprises a positive electrode sheet, an electrolyte, a diaphragm and the above-mentioned aluminum-based composite current collector or the aluminum-based composite current collector prepared by the above-mentioned preparation method.

[0044] The positive electrode sheet comprises a positive electrode active material, a conductive agent and a binder; the electrolyte comprises a sodium salt and an organic solvent.

[0045] Furthermore, the positive electrode active material is any one of sodium vanadium phosphate, sodium iron pyrophosphate, sodium iron pyrophosphate and sodium iron manganese pyrophosphate. For example, the positive electrode active material is sodium vanadium phosphate; the positive electrode active material is sodium iron pyrophosphate; the positive electrode active material is sodium iron pyrophosphate; the positive electrode active material is sodium iron manganese pyrophosphate.

[0046] Furthermore, the conductive agent is any one or more of graphene, carbon nanotubes, acetylene black, Ketjen black or Super P Li. For example, the conductive agent is graphene; the conductive agent is carbon nanotubes; the conductive agent is acetylene black; the conductive agent is Super P Li.

[0047] Furthermore, the binder is polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE). For example, the binder is polyvinylidene fluoride; the binder is polytetrafluoroethylene.

[0048] Further, the sodium salt is any one or more of sodium hexafluorophosphate, sodium perchlorate, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium bis(fluorosulfonyl)imide and sodium bis(trifluoromethylsulfonyl)imide. For example, the sodium salt is sodium hexafluorophosphate; the sodium salt is sodium perchlorate; the sodium salt is sodium trifluoromethanesulfonate; the sodium salt is sodium tetrafluoroborate; the sodium salt is sodium bis(fluorosulfonyl)imide; the sodium salt is sodium bis(trifluoromethylsulfonyl)imide.

[0049] Further, the organic solvent is any one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, diglyme, 1,3-cyclopentanediol, ethylene glycol dimethyl ether and triethylene glycol dimethyl ether. For example, the organic solvent is ethylene carbonate; the organic solvent is propylene carbonate; the organic solvent is dimethyl carbonate; the organic solvent is diethyl carbonate; the organic solvent is diglyme; the organic solvent is 1,3-cyclopentanediol; the organic solvent is ethylene glycol dimethyl ether; the organic solvent is triethylene glycol dimethyl ether.

[0050] Furthermore, the above-mentioned diaphragm is any one of polyethylene, polypropylene microporous membrane, glass fiber membrane and polyacrylonitrile diaphragm. For example, the diaphragm is polyethylene; the diaphragm is polypropylene microporous membrane; the diaphragm is glass fiber membrane; the diaphragm is polyacrylonitrile diaphragm.

[0051] Example 1 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0052] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0053] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 20 s, washed in deionized water, and the immersion-washing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 2 μm. The obtained sample was recorded as “Zn@Al-20”.

[0054] Step 4: Dry the Zn@Al-20 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0055] The invention has a simple manufacturing method and is easy to mass produce. Figure 1 This is an optical image of a zinc-modified aluminum current collector (Example 1) mass-produced by a roll-to-roll chemical plating process. The Zn@Al-20 prepared in Example 1 was subjected to XRD testing. Figure 2 As shown in the figure, the aluminum-based composite current collector is mainly composed of two elements, Zn and Al, and the (101) and (100) crystal planes are the main exposed crystal planes of chemically plated metal Zn. Figure 3 ), the zinc with nanosheet cross-linking structure is evenly distributed on both sides of the aluminum substrate, and the nanoflower-like zinc modification layer is assembled from 1-5 nm thick nanosheets into nanoflowers with a diameter of 100-500 nm. Figure 4The SEM-EDS test results show that the thickness of the zinc layer is 2 microns. The highly ordered porous structure promotes the penetration of electrolyte and the transport of ions. Figure 5 The KPFM results show that the exposed Zn crystal edge of the aluminum-based composite current collector shows a high potential, which increases the regional current density and is beneficial to electron transmission. It has high catalytic activity for the reduction and decomposition of the electrolyte. After the first cycle, a stable SEI is formed on the surface of the current collector, and the coulombic efficiency of the battery is improved. The negative electrode-free sodium-ion battery is assembled with the sodium-based positive electrode material, and the battery achieves stable cycling.

[0056] Example 2 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0057] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0058] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 5 s, washed in deionized water, and the immersion-washing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 0.5 μm. The obtained sample was recorded as “Zn@Al-5”.

[0059] Step 4: Dry the Zn@Al-5 material obtained in step (3) at 60°C for 6 h, and then obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0060] Example 3 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0061] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0062] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 10 s, washed in deionized water, and the immersion-washing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 1 μm. The obtained sample was recorded as “Zn@Al-10”.

[0063] Step 4: Dry the Zn@Al-10 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0064] Example 4 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0065] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0066] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 15 s, rinsed in deionized water, and the immersion-rinsing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 3 μm. The obtained sample was recorded as “Zn@Al-15”.

[0067] Step 4: Dry the Zn@Al-15 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0068] Example 5 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0069] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0070] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 25 s, washed in deionized water, and the immersion-washing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 4 μm. The obtained sample was recorded as “Zn@Al-25”.

[0071] Step 4: Dry the Zn@Al-25 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0072] Example 6 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0073] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0074] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 30 s, washed in deionized water, and the immersion-washing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 5 μm. The obtained sample was recorded as “Zn@Al-30”.

[0075] Step 4: Dry the Zn@Al-30 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0076] Example 7 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 10 s and then soak it in 1.5 M H2SO4 solution for 5 s to remove the oxidized impurities on the Al foil surface.

[0077] Step 2: Dissolve 80 g NaOH and 0.32 g ZnO in 200 mL H2O to prepare a zinc plating solution.

[0078] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 20 s, washed in deionized water, and the immersion-washing process was repeated 5 times to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 2 μm. The obtained sample was recorded as “Zn@Al-20-1”.

[0079] Step 4: Dry the Zn@Al-20-1 material obtained in step (3) at 60°C for 6 h, and then obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0080] Example 8 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the aluminum foil in acetone for 60 s and then soak it in 0.1 M H2SO4 solution for 20 s to remove the oxidized impurities on the surface of the Al foil.

[0081] Step 2: Dissolve 40 g NaOH and 2 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0082] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 5 s, washed in deionized water, and the immersion-washing process was repeated 5 times to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 1.5 μm. The obtained sample was recorded as “Zn@Al-5-1”.

[0083] Step 4: Dry the Zn@Al-5-1 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0084] Example 9 The preparation method of an aluminum-based composite current collector of this embodiment comprises the following steps: Step 1: First, soak the Al foil in acetone for 30 s and then soak it in 1 M H2SO4 solution for 10 s to remove the oxidized impurities on the Al foil surface.

[0085] Step 2: Dissolve 8 g NaOH and 4.8 g ZnO in 200 mL H2O to prepare the zinc plating solution.

[0086] Step 3: The aluminum foil treated in (1) was then immersed in the zinc plating solution for 20 s, washed in deionized water, and the immersion-washing process was repeated twice to deposit a uniform Zn layer on the Al surface. The Zn layer thickness was 2 μm. The obtained sample was recorded as “Zn@Al-20-2”.

[0087] Step 4: Dry the Zn@Al-20-2 material obtained in step (3) at 60°C for 6 h to obtain an aluminum-based composite current collector modified with nanoflower-shaped zinc for a negative electrode-free sodium metal battery.

[0088] Comparative Example 1 In this comparative example, no modification layer is applied to the zinc foil current collector, and the bare zinc foil is directly used as the current collector of the negative electrode-free sodium metal battery, and the thickness of the Zn foil is 20 μm.

[0089] Comparative Example 2 The preparation method of the aluminum-based composite current collector in this comparative example is different from that in Example 1 in that the "slurry stirring-coating" process is adopted for preparation, and the specific steps are as follows: Commercial zinc powder and a binder were weighed in a mass ratio of 9:1 and an appropriate amount of N-methylpyrrolidone solvent was added to prepare a slurry. The prepared slurry was coated on an aluminum foil by blade coating to obtain an aluminum-based composite current collector, wherein the coating thickness was 2 μm.

[0090] Implementation effect example The aluminum-based composite current collectors prepared in Examples 1-9 were used as working electrodes and sodium metal was used as counter electrodes to assemble button cells (half-cells), and the coulombic efficiency and cycle stability of the half-cells were tested. The specific process of assembling the half-cells and testing their performance is as follows: (1) The aluminum-based composite current collectors prepared in Examples 1-9 were respectively dried at 60° C. in a vacuum oven and cut to obtain working electrode sheets with a diameter of 16 mm.

[0091] (2) Sodium metal sheet was used as the counter electrode (13 mm in diameter), glass fiber membrane (Whatman GF / D) was used as the separator, 1 M NaPF6 dissolved in DGM was used as the electrolyte, and stainless steel shell was used as the outer shell to assemble into a CR2025 button cell.

[0092] (3) The half-cell assembled by the above process was charged at room temperature at 1 mA cm -2 The current density and 1 mAh cm -2 The reversibility test of electroplating and stripping was carried out under the condition of sodium deposition amount and charging cut-off voltage of 0.8V. The results of the first week coulombic efficiency and average coulombic efficiency are shown in Table 1.

[0093] Table 1 First week coulombic efficiency and average coulombic efficiency of half-cell As can be seen from Table 1, the first cycle coulombic efficiency of the aluminum-based composite current collectors prepared in Examples 1-9 is about 74%-98%, and the average coulombic efficiency is about 95%-99.94%. The one prepared in Example 1 exhibits the best cycle performance.

[0094] Figure 6 The figure is a cycle stability diagram of the coulombic efficiency of the half-cell with Examples 1-6 as the working electrode and sodium as the counter electrode. It can be seen that when Examples 2-6 are used as current collectors, the coulombic efficiency fluctuates greatly, indicating that the reversibility of the deposition and dissolution process of sodium metal is poor. However, when the current collector of Example 1 is used, the coulombic efficiency is very stable, and the average coulombic efficiency reaches more than 99.9%, indicating that the reversibility of sodium deposition and dissolution is high and the amount of sodium that loses activity is small, indicating that the nanoflower-shaped zinc-modified aluminum-based composite current collector has the potential to be used in negative-electrode-free sodium metal batteries.

[0095] Depend on Figure 7 It can be seen that after the first cycle of the half-cell, the aluminum-based composite current collector after the cycle was taken out for TEM testing. The test results showed that the surface of the aluminum-based current collector after the cycle was covered with a uniform SEI with a thickness of about 18 nm. At the same time, different lattice fringes can be observed in the corresponding area under high resolution, and the corresponding crystal components can be clearly identified by Fourier transform as Na2CO3, NaF, ZnF2 and NaZn13 Therefore, after the first cycle of the battery, a uniform, thin, and inorganic SEI is formed on the surface of the aluminum-based composite current collector. This helps the negative electrode-free sodium battery achieve high coulombic efficiency and excellent cycle life.

[0096] The half-cell assembled with the aluminum-based composite current collector prepared in Example 1 was heated at room temperature at 3 mA cm -2 The current density and 3 mAh cm -2 The reversibility test of electroplating and stripping was carried out under the condition of sodium deposition and charging cut-off voltage of 0.8V. The results of the first week coulomb efficiency and average coulomb efficiency are shown in the figure. Figure 8 The results show that the current collector of Example 1 can -2 and high surface capacity 3 mAh cm -2 In the next cycle, the coulombic efficiency is very stable, and the average coulombic efficiency reaches more than 99.9%, indicating that the reversibility of sodium deposition and dissolution is high and the amount of sodium that loses activity is small, indicating that the nanoflower-like zinc-modified aluminum-based composite current collector has the potential to be used in negative electrode-free sodium metal batteries.

[0097] In order to further explore the influence of aluminum-based composite current collector on the dendrite inhibition and cycle life of batteries when applied to batteries, the following batteries (symmetrical batteries) were assembled and their performance was tested.

[0098] The sodium metal sheet was pressed onto the aluminum-based composite current collector prepared in Example 1 as the working electrode and the counter electrode of the battery, respectively, and assembled into a button-type battery (symmetrical battery). The dendrite inhibition effect and cycle life of the symmetrical battery were tested. The specific test process of the assembly and performance of the symmetrical battery is as follows: (1) The aluminum-based composite current collectors prepared in Example 1 were vacuum dried at 60° C. and cut into pieces with a diameter of 16 mm; (2) Press a sodium metal sheet (13 mm in diameter) onto the aluminum-based composite current collector cut in the first step to prepare a pole piece; (3) The electrodes prepared in the second step were used as the working electrode and the counter electrode, respectively, the glass fiber membrane (Whatman GF / D) was used as the diaphragm, 1 M NaPF6 dissolved in DGM was used as the electrolyte, and the stainless steel shell was used as the outer shell to assemble into a CR2025 button battery.

[0099] (4) The symmetrical battery assembled by the above process was heated at room temperature at 1, 2, and 3 mA cm -2 The current density and 1, 2, and 3 mAh cm -2 Under the condition of sodium deposition, the dendrite inhibition and cycle life tests were carried out. The test results are as follows Fig. 9As shown in the figure, at currents of 1, 2, and 3 mA cm -2 and high surface capacities of 1, 2, 3 mAh cm -2 In the next cycle, the symmetric batteries all achieved a stable cycle of more than 1000 hours. The sodium-philic Zn layer effectively promoted the uniform distribution of sodium ions on the current collector, regulated the uniform nucleation and subsequent stable growth of sodium metal, inhibited dendrite growth and buffered volume expansion, indicating that the nanoflower-like zinc-modified aluminum-based composite current collector has the potential to be used in negative electrode-free sodium metal batteries.

[0100] Application Example 1 The aluminum-based composite current collector prepared in Example 1 is used to prepare a negative electrode-free sodium battery, and the steps are as follows: (1) The positive electrode active material (sodium vanadium phosphate), binder PVDF, and conductive agent Super P Li were dissolved in N-methylpyrrolidone solvent at a mass ratio of 7:2:1 and stirred evenly to prepare a slurry. The slurry was applied on the current collector and dried overnight at 120°C in vacuum. Then, a 12 mm pole piece was punched and the pole piece loading was 32 mg cm -2 Made into positive electrode sheet.

[0101] (2) The aluminum-based composite current collector prepared in Example 1 was punched into a pole piece (with a diameter of 16 mm), a glass fiber membrane (Whatman GF / D) was used as a separator, 80 mL of 1 M electrolyte (sodium salt is sodium hexafluorophosphate (NaPF6)), and the organic solvent is diethylene glycol dimethyl ether (DGM)) was added dropwise. A stainless steel shell was used as the outer shell to assemble a CR2025 button battery.

[0102] (3) The sodium ion battery assembled by the above process was charged and discharged at room temperature in the potential range of 2.5-3.8V. The charge and discharge curves and cycle performance are shown in Figure 2. Fig.10 shown. Fig.10 It can be seen that at a current density of 0.1C, the capacity retention rate of the negative electrode-free sodium battery assembled with the zinc foil current collector prepared in Example 1 was 86% after 90 stable cycles, and the coulombic efficiency also reached more than 99%. Fig.10 b It can be seen that the trend of the charge-discharge curve of the battery after 90 cycles remains almost unchanged compared with the first cycle, which proves that the loss of active substances in the positive electrode material is small and the active substances in the material are well maintained. This further confirms the application potential of the composite current collector of Example 1 in negative electrode-free sodium metal batteries.

[0103] Application Example Comparative Example 1 A negative electrode-free sodium battery was prepared using the zinc foil current collector prepared in Comparative Example 1, and the steps were as follows: (1) The positive electrode active material (sodium vanadium phosphate), binder PVDF, and conductive agent Super P Li were dissolved in N-methylpyrrolidone solvent at a mass ratio of 7:2:1 and stirred evenly to prepare a slurry. The slurry was applied on the current collector and dried overnight at 120°C in vacuum. Then, a 12 mm pole piece was punched and the pole piece loading was 32 mg cm -2 Made into positive electrode sheet.

[0104] (2) The zinc foil current collector of comparative example 1 was punched into a pole piece (diameter 16 mm), a glass fiber membrane (Whatman GF / D) was used as a separator, 80 mL of 1 M electrolyte (sodium salt is sodium hexafluorophosphate (NaPF6)), and the organic solvent is diethylene glycol dimethyl ether (DGM)) was added dropwise. A stainless steel shell was used as the outer shell to assemble a CR2025 button battery.

[0105] (3) The sodium ion battery assembled by the above process was charged and discharged at room temperature in the potential range of 2.5-3.8V. The charge and discharge curves and cycle performance are shown in Figure 2. Fig.11 shown. Fig.11 It can be seen that at a current density of 0.1C, the discharge capacity of the negative electrode-free sodium battery assembled with the zinc foil current collector prepared in Comparative Example 1 continued to decrease during the entire cycle, and the discharge capacity was almost zero after 100 cycles. Fig.11 b It can be seen that the discharge capacity in the first week is much lower than the theoretical capacity of the active material, and the trend of the charge and discharge curve after the battery is cycled for 90 weeks is completely inconsistent with that of the first cycle, which proves that the active material loss of the positive electrode material is serious.

[0106] Application Example Comparative Example 2 The negative electrode-free sodium battery was prepared using the aluminum-based composite current collector prepared in Comparative Example 2, and the steps are as follows: (1) The positive electrode active material (sodium vanadium phosphate), binder PVDF, and conductive agent Super P Li were dissolved in N-methylpyrrolidone solvent at a mass ratio of 7:2:1 and stirred evenly to prepare a slurry. The slurry was applied on the current collector and dried overnight at 120°C in vacuum. Then, a 12 mm pole piece was punched and the pole piece loading was 32 mg cm -2 Made into positive electrode sheet.

[0107] (2) The aluminum-based composite current collector prepared in Comparative Example 2 was punched into a pole piece (with a diameter of 16 mm), a glass fiber membrane (Whatman GF / D) was used as a separator, 80 mL of 1 M electrolyte (sodium salt is sodium hexafluorophosphate (NaPF6)), and the organic solvent is diethylene glycol dimethyl ether (DGM)) was added dropwise. A stainless steel shell was used as the outer shell to assemble a CR2025 button battery.

[0108] (3) The sodium ion battery assembled by the above process was charged and discharged at room temperature in the potential range of 2.5-3.8V. The charge and discharge curves and cycle performance are shown in Figure 2. Fig.12 shown. Fig.12 It can be seen from a that at a current density of 0.1C, the discharge capacity of the negative electrode-free sodium battery assembled with the aluminum-based composite current collector prepared in Comparative Example 2 continued to decrease during the entire cycle, and the discharge capacity became zero after 15 cycles. Fig.12 b It can be seen that the discharge capacity in the first week is much lower than the theoretical capacity of the active material, and the trend of the charge and discharge curve after the battery is cycled for 15 weeks is completely inconsistent with that of the first cycle, which proves that the active material loss of the positive electrode material is serious.

[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An aluminum-based composite current collector, characterized in that: The invention comprises an aluminum foil and a nano-flower-shaped zinc modification layer. The nano-flower-shaped zinc modification layer is composed of nano-sheets with a thickness of 1-5 nm and nano-flowers with a diameter of 100-500 nm. The thickness of the nano-flower-shaped zinc modification layer is 0.5-5 μm.

2. The method for preparing the aluminum-based composite current collector according to claim 1, characterized in that: Here are the steps: (1) Pre-treating the aluminum foil; (2) Sodium hydroxide and zinc oxide are dissolved in deionized water to prepare a zinc plating solution, and then the aluminum foil pretreated in step (1) is immersed in the zinc plating solution, and then washed with deionized water. After repeating the immersion-washing process 2-5 times, the aluminum-based composite current collector is obtained after drying.

3. The method for preparing the aluminum-based composite current collector according to claim 1, characterized in that: The pretreatment in step (1) includes acetone treatment and H2SO4 solution treatment.

4. The method for preparing the aluminum-based composite current collector according to claim 3, characterized in that: The acetone treatment refers to acetone ultrasonic cleaning for 10-60 s; the H2SO4 solution treatment refers to 0.1-1.5 M sulfuric acid treatment for 5-20 s.

5. The method for preparing the aluminum-based composite current collector according to claim 3, characterized in that: In the step (2), the concentration of sodium hydroxide in the zinc plating solution is 1-10 mol / L, and the concentration of zinc oxide is 0.02-0.3 mol / L.

6. The method for preparing the aluminum-based composite current collector according to claim 5, characterized in that: The time of immersion in the zinc plating solution in step (2) is 5-30 s.

7. Use of the aluminum-based composite current collector according to claim 1 in a negative electrode-free sodium battery.

8. A negative electrode-free sodium battery, characterized in that: The invention comprises a positive electrode sheet, an electrolyte, a separator and the aluminum-based composite current collector according to claim 1 or the aluminum-based composite current collector prepared by the preparation method according to any one of claims 2 to 6.

9. The negative electrode-free sodium battery according to claim 8, characterized in that: The positive electrode sheet includes a positive electrode active material, a conductive agent and a binder; the electrolyte includes a sodium salt and an organic solvent.

10. The negative electrode-free sodium battery according to claim 9, characterized in that: The positive electrode active material is any one of sodium vanadium phosphate, sodium ferric pyrophosphate, sodium ferric pyrophosphate and sodium manganese ferric pyrophosphate; the conductive agent is any one or more of graphene, carbon nanotubes, acetylene black, Ketjen black or Super P Li; the binder is polyvinylidene fluoride or polytetrafluoroethylene; the sodium salt is any one or more of sodium hexafluorophosphate, sodium perchlorate, sodium trifluoromethylsulfonate, sodium tetrafluoroborate, sodium bis(fluorosulfonyl)imide and sodium bis(trifluoromethylsulfonyl)imide; the organic solvent is any one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, diethylene glycol dimethyl ether, 1,3-cyclopentanediol, ethylene glycol dimethyl ether and triethylene glycol dimethyl ether; the diaphragm is any one of polyethylene, polypropylene microporous membrane, glass fiber membrane and polyacrylonitrile diaphragm.

Citation Information

Cited By

  • Surface modified aluminum foil current collector, preparation method thereof and sodium ion battery

    CN119965278A

  • Composite current collector, preparation method and application thereof, and negative-electrode-free sodium ion battery

    CN120015842A

  • Aluminum foil for negative-electrode-free sodium battery and preparation method of aluminum foil

    CN120536779A

  • Negative-electrode-free sodium ion battery current collector, preparation method and application thereof, and negative-electrode-free sodium ion battery

    CN120600830A

  • Negative current collector, preparation method thereof and sodium ion battery

    CN121862759A