High-spinnability polyacrylonitrile spinning solution and preparation method thereof
By introducing sulfonic acid-based and olefin-based long-chain benzene comonomers into the polyacrylonitrile spinning stock solution, the problem of poor hydrophilicity of the polyacrylonitrile copolymer is solved, the spinnability and mechanical properties of the carbon fiber are improved, and the Low-cost and efficient preparation of spinning dope, suitable for the production of multifunctional carbon fibers.
Patent Information
- Application Number
- CN202411008808.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The hydrophilicity of polyacrylonitrile copolymers in the prior art is poor, resulting in insufficient spinnability and mechanical properties of carbon fibers, and excessive comonomer components can lead to structural defects and reduced mechanical properties of carbon fibers.
Using acrylonitrile monomer, sulfonic acid monomer and olefin-based long-chain benzene as comonomers, through solution polymerization and the use of initiators, a highly spinnable polyacrylonitrile spinning stock solution is prepared, utilizing the volume of side groups The effect reduces the cohesive energy of polyacrylonitrile copolymer and improves the spinnability and mechanical properties of carbon fiber.
It improves the spinnability and mechanical properties of carbon fiber, reduces the exothermic reaction during pre-oxidation and cyclization, controls structural transformation, has low cost and simple process, and is suitable for large-scale industrial production.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of carbon fibers, and particularly relates to a high-spinnability polyacrylonitrile spinning solution and a preparation method thereof. Background Art
[0002] Carbon fiber is an inorganic fibrous material in which incomplete flake graphite crystals with a carbon content of more than 90% are stacked along the fiber axis. Carbon fiber has many advantages, such as high strength and modulus, good heat resistance, chemical stability and dimensional stability, and small linear expansion coefficient. It is an important industrial fiber at present and is often used as a reinforcement and insulation material for various composite materials such as carbon, resin, and ceramic. The mechanical properties of carbon fiber are almost unaffected by high temperatures. It was first used in the fields of national defense and aerospace, and plays a vital role in the development of the country. The application of carbon fiber in the field of sports and leisure products, such as bicycles, fishing rods, tennis rackets, golf clubs, and yachts, accounts for about 16% of its total consumption. In addition, the global demand for polyacrylonitrile-based carbon fiber is still growing.
[0003] The quality of carbon fiber is directly affected by the structure and performance of the precursor, and the performance of polyacrylonitrile carbon fiber precursor is closely related to the preparation of spinning solution. In terms of preparation technology, the preparation of existing carbon fiber spinning solution mostly adopts binary or ternary copolymerization. This is because the homopolymerized acrylonitrile polymer has strong rigidity, resulting in poor spinnability of the solution. The heat release in the later pre-oxidation and carbonization process will also be too concentrated, causing the fiber to break easily during the oxidation and carbonization drawing process, reducing the mechanical properties of the carbon fiber. Therefore, comonomers are usually used to improve the spinnability of polyacrylonitrile solution and alleviate the heat release during the oxidation and carbonization process.
[0004] Chinese patent CN202110434140.X (publication date October 25, 2022) discloses a polymer for polyacrylonitrile-based large-tow carbon fiber, a preparation method, and polyacrylonitrile-based large-tow carbon fiber. The invention introduces a fourth comonomer, a long-chain fatty acid ester, which reduces the cohesive energy of the molecular weight of the polyacrylonitrile copolymer and improves the spinnability. Although this method can effectively improve the spinnability of polyacrylonitrile, the excessive components in the comonomer are not conducive to the formation of annular graphite-like structures during the preparation of carbon fiber. The introduction of long-chain fatty acid esters as the fourth comonomer will increase the structural defects of the carbon fiber, resulting in reduced mechanical properties of the carbon fiber.
[0005] Chinese patent CN201010191644.5 (publication date October 20, 2010) discloses a method for preparing a hydrophilic spinning solution of polyacrylonitrile-based carbon fiber, which adopts a more hydrophilic monomethyl itaconate ammonium compound to replace monomethyl itaconate as a comonomer to obtain a spinning solution with a higher hydrophilicity than monomethyl itaconate. Although this method can avoid the problem of loose coagulation fiber structure caused by the increase in the difference in diffusion rate between the solvent and the non-solvent in the fiber due to the decrease in the hydrophilicity of the spinning solution, the monomethyl itaconate ammonium compound is an ionic liquid, and the production cost is high, which is not conducive to subsequent large-scale industrial production. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a high-spinnability polyacrylonitrile spinning solution and a preparation method thereof, so as to overcome the defect of poor hydrophilicity of polyacrylonitrile copolymer in the prior art.
[0007] The present invention provides a high-spinnability polyacrylonitrile spinning solution, the spinning solution comprises acrylonitrile monomer, a second comonomer and a third comonomer; wherein the second comonomer is a sulfonic acid monomer; and the third comonomer is an olefin-based long-chain benzene.
[0008] Preferably, the sulfonic acid monomer is at least one of 2-sulfofumaric acid (24674-75-7), (Z)-3-sulfo-2-acrylic acid (875610-90-5), (E)-3-sulfo-2-acrylic acid (875610-88-1) or 2-sulfo-2-butenedioic acid (65319-67-7).
[0009] Preferably, the olefin-based long-chain benzene is at least one of 4-n-octylstyrene, 4-isobutylstyrene, 2-methyl-4-n-butylstyrene, 2-n-pentylstyrene, 3-n-butylstyrene and 1-methyl-5-n-butylstyrene.
[0010] Preferably, the mass content of acrylonitrile monomer in the spinning solution is 90%-99%, more preferably 95%-98%; the mass content of the second comonomer is 1%-8%, more preferably 1.5%-4%; the mass content of the third comonomer is 1%-8%, more preferably 1%-4%.
[0011] The present invention also provides a method for preparing a high-spinnability polyacrylonitrile spinning solution, comprising the following steps:
[0012] The acrylonitrile monomer, the second comonomer, the third comonomer and the initiator are subjected to solution polymerization in a solvent, and residual monomers and bubbles are removed to obtain a high-spinnability polyacrylonitrile spinning solution.
[0013] Preferably, the initiator is at least one of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate and ammonium persulfate; the amount of the initiator used is 0.2% to 0.5% of the amount of acrylonitrile used, preferably 0.2% to 0.4%.
[0014] Preferably, the solvent is at least one of dimethyl sulfoxide, dimethylformamide and dimethylacetamide.
[0015] Preferably, the solution polymerization is carried out under a nitrogen atmosphere at a temperature of 45 to 65° C., preferably 50 to 65° C., for a time of 6 to 40 hours, preferably 10 to 25 hours.
[0016] Preferably, the process for removing residual monomers is: distilling the solution under the protection of nitrogen, and controlling the residual monomer content to be below 0.15%.
[0017] Preferably, the process for removing bubbles is as follows: pressure of 8 to 25 KPa, temperature of 30 to 100° C., and time of 2 to 5 days.
[0018] The invention is based on the binary copolymerization of acrylonitrile and sulfonic acid monomers, and introduces a third comonomer, olefin-based long-chain benzene, and utilizes the volume effect of the side group to reduce the cohesive energy of the molecular weight of the polyacrylonitrile copolymer, so as to achieve the purpose of improving the spinnability of the polyacrylonitrile-based carbon fiber. The invention has the advantages of low cost, good pre-oxidation cyclization performance, easy reaction control, good hydrophilicity, and the like.
[0019] Beneficial Effects
[0020] (1) The present invention introduces a sulfonic acid group-containing acrylic monomer. The sulfonic acid group can weaken the intramolecular and intermolecular dipole interaction force of the cyano group in the polyacrylonitrile molecule, thereby reducing the activation energy of the fiber reaction when preparing carbon fiber, which is beneficial to promote cyclization and cross-linking, improve the density and uniformity of the fiber, reduce the chance of main chain breakage, and ensure the strength of the carbon fiber.
[0021] (2) The present invention improves the pre-oxidation process of PAN precursor by introducing the third comonomer, so that the cyclization reaction can be initiated at a lower temperature. In addition, the introduction of the third comonomer makes the propagation reaction present an ionic mechanism, which alleviates the exothermic reaction in the pre-oxidation process and makes it easier to control the pre-oxidation process and structural transformation.
[0022] (3) The third comonomer used in the present invention is an olefin-based long-chain benzene, which has an active carbon-carbon double bond and is conducive to forming copolymers with various olefin monomers. The volume effect of the aromatic side group can be used to reduce the cohesive energy in the polyacrylonitrile copolymer molecules, so as to achieve the purpose of improving the spinnability of polyacrylonitrile-based carbon fibers.
[0023] (4) The present invention has low cost and simple preparation process. The contact angle of the obtained spinning solution with water after film formation can reach 35° to 50°, and the hydrophilicity of the polymer chain is greatly improved, which is suitable for preparing multifunctional polyacrylonitrile-based carbon fiber precursor. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0025] Comparative Example 1
[0026] Solvent dimethyl sulfoxide, main monomer acrylonitrile, second comonomer 2-sulfofumaric acid, free radical initiator azobisisobutyronitrile are added to a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 98% of the total weight of the monomer, the second comonomer 2-sulfofumaric acid is 2% of the total weight of the monomer, the amount of azobisisobutyronitrile is 0.75% of the total weight of the monomer, and the total monomer concentration is 25%. The mixture is stirred and mixed at room temperature, and after nitrogen bubbling for 20 minutes, it is kept at 65°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under the protection of nitrogen, and the residual monomer content is controlled to be below 0.15%. The process for removing bubbles is: the pressure is 8KPa, the temperature is 30°C, and the time is 5 days. The weight average molecular weight of the spinning solution is 271,000, and the contact angle with water after film formation is 51.6°.
[0027] Example 1
[0028] Solvent dimethyl sulfoxide, main monomer acrylonitrile, second comonomer 2-sulfonic acid-2-butenedioic acid, free radical initiator azobisisobutyronitrile are added to a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 97% of the total weight of the monomer, the second comonomer 2-sulfonic acid-2-butenedioic acid is 3% of the total weight of the monomer, the amount of azobisisobutyronitrile is 0.75% of the total weight of the monomer, and the total monomer concentration is 25%. The mixture is stirred and mixed at room temperature, and after nitrogen bubbling for 20 minutes, it is kept at 65°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under the protection of nitrogen, and the residual monomer content is controlled to be below 0.15%. The process for removing bubbles is: the pressure is 8KPa, the temperature is 40°C, and the time is 5 days. The weight average molecular weight of the spinning solution is 265,000, and the contact angle with water after film formation is 40.0°.
[0029] Example 2
[0030] Solvent dimethyl sulfoxide, main monomer acrylonitrile, second comonomer 2-sulfofumaric acid and third comonomer 4-n-octylstyrene, free radical initiator azobisisobutyronitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 98% of the total weight of the monomers, the second comonomer 2-sulfofumaric acid is 1% of the total weight of the monomers, the third comonomer 4-n-octylstyrene is 1% of the total weight of the monomers, the amount of azobisisobutyronitrile is 0.75% of the total weight of the monomers, and the total monomer concentration is 25%. The mixture is stirred and mixed at room temperature, and after nitrogen bubbling for 20 minutes, it is kept at 65°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under the protection of nitrogen, and the residual monomer content is controlled to be below 0.15%. The process of removing bubbles is as follows: pressure of 10 KPa, temperature of 50°C, and time of 4 days. The weight average molecular weight of the spinning solution is 242,000, and the contact angle with water after film formation is 38.0°.
[0031] Example 3
[0032] Solvent dimethyl sulfoxide, main monomer acrylonitrile, second comonomer 2-sulfofumaric acid and third comonomer 4-n-octylstyrene, free radical initiator azobisisobutyronitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 99% of the total weight of the monomers, the second comonomer 2-sulfofumaric acid is 0.75% of the total weight of the monomers, the third comonomer 4-n-octylstyrene is 0.25% of the total weight of the monomers, and the amount of azobisisobutyronitrile is 0.25% of the total weight of the monomers, and the total monomer concentration is 23.5%. The mixture is stirred and mixed at room temperature, and after nitrogen bubbling for 20 minutes, it is kept at 50°C for 36 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under the protection of nitrogen, and the residual monomer content is controlled to be below 0.15%. The process of removing bubbles is as follows: pressure of 15 KPa, temperature of 60°C, and time of 4 days. The weight average molecular weight of the spinning solution is 562,000, and the contact angle with water after film formation is 46.0°.
[0033] Example 4
[0034] Solvent dimethyl sulfoxide, main monomer acrylonitrile, second comonomer 2-sulfofumaric acid and third comonomer 4-n-octylstyrene, free radical initiator azobisisobutyronitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 90% of the total weight of the monomers, the second comonomer 2-sulfofumaric acid is 5% of the total weight of the monomers, the third comonomer 4-n-octylstyrene is 5% of the total weight of the monomers, the amount of azobisisobutyronitrile is 0.5% of the total weight of the monomers, and the total monomer concentration is 20%. The mixture is stirred and mixed at room temperature, nitrogen is bubbled for 20 minutes, and then the mixture is kept at 60°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under the protection of nitrogen, and the residual monomer content is controlled to be below 0.15%. The process of removing bubbles is as follows: pressure of 18 KPa, temperature of 65°C, and time of 3 days. The weight average molecular weight of the spinning solution is 104,000, and the contact angle with water after film formation is 34.5°.
[0035] Example 5
[0036] Solvent dimethylformamide, main monomer acrylonitrile, second comonomer (Z)-3 sulfo-2-acrylic acid and third comonomer 2-methyl-4-n-butylstyrene, free radical initiator azobisisobutyronitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 97% of the total weight of the monomers, the second comonomer (Z)-3 sulfo-2-acrylic acid is 1.5% of the total weight of the monomers, the third comonomer 2-methyl-4-n-butylstyrene is 1.5% of the total weight of the monomers, the amount of azobisisobutyronitrile is 0.75% of the total weight of the monomers, and the total monomer concentration is 20%. The mixture is stirred and mixed at room temperature, and after nitrogen bubbling for 20 minutes, it is kept at 60°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under nitrogen protection, and the residual monomer content is controlled to be below 0.15%. The process of removing bubbles is as follows: pressure of 20 KPa, temperature of 50°C, and time of 3 days. The weight average molecular weight of the spinning solution is 243,000, and the contact angle with water after film formation is 47.5°.
[0037] Example 6
[0038] Solvent dimethylformamide, main monomer acrylonitrile, second comonomer (Z)-3 sulfo-2-acrylic acid and third comonomer 2-n-pentylstyrene, free radical initiator azobisisovaleronitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: the main monomer acrylonitrile is 97% of the total weight of the monomers, the second comonomer (Z)-3 sulfo-2-acrylic acid is 1.5% of the total weight of the monomers, the third comonomer 2-n-pentylstyrene is 1.5% of the total weight of the monomers, the amount of azobisisovaleronitrile is 0.75% of the total weight of the monomers, and the total monomer concentration is 20%. The mixture is stirred and mixed at room temperature, nitrogen is bubbled for 20 minutes, and then the mixture is kept at 60°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under nitrogen protection, and the residual monomer content is controlled to be below 0.15%. The process of removing bubbles is as follows: pressure of 20 KPa, temperature of 70°C, and time of 3 days. The weight average molecular weight of the spinning solution is 234,000, and the contact angle with water after film formation is 47.0°.
[0039] Example 7
[0040] Solvent dimethylformamide, main monomer acrylonitrile, second comonomer (E)-3-sulfo-2-acrylic acid and third comonomer 4-isobutylstyrene, free radical initiator azobisisovaleronitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: main monomer acrylonitrile is 97% of the total weight of monomers, second comonomer (E)-3-sulfo-2-acrylic acid is 1.5% of the total weight of monomers, third comonomer 4-isobutylstyrene is 1.5% of the total weight of monomers, and the amount of azobisisovaleronitrile is 0.75% of the total weight of monomers, and the total concentration of monomers is 20%. The mixture is stirred and mixed at room temperature, and nitrogen is bubbled for 20 minutes. Under nitrogen protection, it is kept at 60°C for 24 hours, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process for removing the residual monomers is: distilling the solution under nitrogen protection, and the residual monomer content is controlled to be below 0.15%. The process of removing bubbles is as follows: pressure of 22 KPa, temperature of 80°C, and time of 2 days. The weight average molecular weight of the spinning solution is 276,000, and the contact angle with water after film formation is 46.5°.
[0041] Example 8
[0042] Solvent dimethylformamide, main monomer acrylonitrile, second comonomer 2-sulfonic acid-2-butenedioic acid and third comonomer 1-methyl-5-n-butylstyrene, free radical initiator azobisisoheptylnitrile are added into a reactor with a condenser and a mechanical stirring device. The weight percentage ratio of the added raw materials is: main monomer acrylonitrile is 97% of the total weight of the monomers, second comonomer 2-sulfonic acid-2-butenedioic acid is 1.5% of the total weight of the monomers, third comonomer 1-methyl-5-n-butylstyrene is 1.5% of the total weight of the monomers, and the amount of azobisisoheptylnitrile is 0.75% of the total weight of the monomers, and the total monomer concentration is 20%. The mixture is stirred and mixed at room temperature, nitrogen is bubbled for 20 minutes, and then the mixture is kept at 60°C for 24 hours under nitrogen protection, and then the residual monomers and bubbles are removed to obtain a high spinnability polyacrylonitrile spinning solution. The process of removing residual monomers is: distilling the solution under the protection of nitrogen, and the residual monomer content is controlled below 0.15%. The process of removing bubbles is: pressure 25KPa, temperature 100°C, time 2 days. The weight average molecular weight of the spinning solution is 298,000, and the contact angle with water after film formation is 45.5°.
[0043] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A high-spinnability polyacrylonitrile spinning solution, Features: The spinning solution comprises acrylonitrile monomer, a second comonomer and a third comonomer; wherein the second comonomer is a sulfonic acid monomer; and the third comonomer is an olefin-based long-chain benzene.
2. The high spinnability polyacrylonitrile spinning solution according to claim 1, Features: The sulfonic acid monomer is at least one of 2-sulfofumaric acid, (Z)-3-sulfo-2-acrylic acid, (E)-3-sulfo-2-acrylic acid or 2-sulfo-2-butenedioic acid.
3. The high spinnability polyacrylonitrile spinning solution according to claim 1, Features: The olefin-based long-chain benzene is at least one of 4-n-octylstyrene, 4-isobutylstyrene, 2-methyl-4-n-butylstyrene, 2-n-pentylstyrene, 3-n-butylstyrene and 1-methyl-5-n-butylstyrene.
4. The high spinnability polyacrylonitrile spinning solution according to claim 1, Features: The mass content of acrylonitrile monomer in the spinning solution is 90%-99%, the mass content of the second comonomer is 1%-8%, and the mass content of the third comonomer is 1%-8%.
5. A method for preparing the high spinnability polyacrylonitrile spinning solution according to any one of claims 1 to 4, comprising the following steps: The acrylonitrile monomer, the second comonomer, the third comonomer and the initiator are subjected to solution polymerization in a solvent, and residual monomers and bubbles are removed to obtain a high-spinnability polyacrylonitrile spinning solution.
6. The preparation method according to claim 5, Features: The initiator is at least one of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate and ammonium persulfate; the dosage of the initiator is 0.2% to 0.5% of the dosage of acrylonitrile.
7. The preparation method according to claim 5, Features: The solvent is at least one of dimethyl sulfoxide, dimethylformamide and dimethylacetamide.
8. The preparation method according to claim 5, Features: The total concentration of the acrylonitrile monomer, the second comonomer and the third comonomer is 20%-25%.
9. The preparation method according to claim 5, Features: The solution polymerization is carried out in a nitrogen atmosphere at a temperature of 45 to 65° C. for a time of 6 to 40 hours.
10. The preparation method according to claim 5, Features: The process for removing residual monomers is: distilling the solution under the protection of nitrogen, and controlling the residual monomer content below 0.15%; the process for removing bubbles is: pressure of 8-25KPa, temperature of 30-100°C, and time of 2-5 days.
Citation Information
Patent Citations
Preparation method of high-solid-content polyacrylonitrile-based carbon fiber spinning solution with controllable viscosity
CN104562222A
Method for producing acrylic fiber
CN107250449A
Novel polyacrylonitrile multipolymer and method for preparing spinning solution of novel polyacrylonitrile multipolymer
CN108586658A
Acrylic shrinkable fiber and process for producing the same
CN1985031A
Acrylonitrile composition
WO2024116994A1