Synthetic method of polyethylene glycol terephthalate
Through the 'deacetic acid' transesterification polymerization of terephthalic acid and ethylene glycol diacetate, the problems of diethylene glycol generation and EG side reactions in the direct esterification method are solved, and high molecular weight, oxidation-resistant PET polymerization is obtained material and realize the reuse of EGDA, providing a new PET synthesis idea.
Patent Information
- Application Number
- CN202310361484.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-03
AI Technical Summary
In the current production of PET polyester, the direct esterification method leads to an increase in the production of diethylene glycol due to the solubility problem of TPA, which affects the quality of the polyester. In addition, the side reaction of EG produces impurities, which reduces the oxidation resistance and light resistance of the polyester. At the same time, EG is difficult to reuse.
Using terephthalic acid and ethylene glycol diacetate as polymerization raw materials, polymerization is carried out through the 'deacetic acid' transesterification method to avoid undesired condensation methods. EGDA is used to replace EG to improve the oxygen resistance of the reaction and control the reaction conditions. and catalyst selection to achieve efficient PET polymerization.
The obtained PET polymer has a high molecular weight, improved oxidation resistance and yellowing resistance. EGDA is easier to detach and can be reused without impurities. It provides a new PET synthesis route and improves product quality and production efficiency.
Smart Images

Figure CN118772383A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a novel synthesis method of polyethylene terephthalate. By using the method, polyethylene terephthalate can be obtained by taking terephthalic acid and ethylene glycol diacetate as polymerization raw materials, and belongs to the field of polymer chemistry. Background Art
[0002] Polyethylene terephthalate (PET) is a high-strength, high-modulus thermoplastic resin with many excellent mechanical properties. It is also resistant to chemical corrosion and has a very low permeability to oxygen and water. Therefore, it is widely used in various containers, food packaging materials, textile industry, civil construction and other fields.
[0003] When PET polyester plastics were just being vigorously developed, the quality of terephthalic acid (TPA) was difficult to meet the requirements for the production of PET polyester due to the immature purification technology of terephthalic acid (TPA). Therefore, a method was developed to convert TPA into dimethyl terephthalate (DMT) which is easy to purify and refine through esterification, and then the refined DMT was transesterified with ethylene glycol (EG) to synthesize polyester. Since the breakthrough in the refining process of TPA in the 1960s, the direct esterification method of TPA and EG has developed rapidly. Since the direct esterification method has more advantages than the transesterification method (less raw material consumption, smaller EG recovery system, no methanol by-product, safer production, shorter production process, lower cost, etc.), the synthesis production lines of newly built PET polyester production plants have turned to the direct polymerization method. At present, more than 75% of the world's PET is produced by the direct esterification method.
[0004] Direct esterification method, that is, using high-purity TPA as the polymerization raw material and esterifying it with EG under nitrogen protection, and then continuously polycondensing it into PET polyester under high vacuum. Since the solubility of TPA in EG is not large, it is often necessary to add excessive EG, which greatly increases the chance of generating diethylene glycol. In the polyester industry, the content of diethylene glycol is an important control indicator affecting the quality of polyester products. The presence of diethylene glycol will reduce the melting point and softening point of polyester, and the oxidation resistance and light resistance of polyester will deteriorate. In addition, the evaporated EG is prone to side reactions, producing impurities such as diethylene glycol and 1,4-dioxane, which makes EG unable to be directly reused. Summary of the invention
[0005] The present invention aims to provide a new synthesis method of polyethylene terephthalate, that is, using TPA and EGDA as polymerization raw materials, under the action of a catalyst, polymerizing PET polymer through a "deacetic acid" transesterification method. In the "deacetic acid" transesterification method, both ends of the ethylene glycol segment in EGDA are capped by acetyl groups, and there are no free active hydroxyl species, so there will be no undesirable condensation mode (such as forming diethylene glycol segments) in the polymerization process to affect the polymer properties; and because EG is not used, the tolerance to oxygen in the reaction process is stronger, and the produced PET will be more resistant to oxidation and yellowing. On the other hand, the boiling point of EGDA is lower than that of EG, so in theory EGDA is easier to leave the system, and the evaporated EGDA has no other impurities and can be directly used for the next polymerization.
[0006] The synthetic method of polyethylene terephthalate of the present invention comprises the following steps:
[0007] Terephthalic acid, ethylene glycol diacetate and a catalyst are mixed in a polyester reactor, the air in the reactor is replaced by an inert gas, and finally a certain pressure is maintained in the polyester reactor, and then the temperature begins to rise. The first stage of the transesterification reaction occurs at 240-280°C, and the pressure is always controlled at about 4-10atm. The progress of the transesterification reaction is evaluated by the yield of the by-product acetic acid. After the transesterification reaction is completed, the second stage of the polycondensation reaction occurs at 270-290°C and a high vacuum of less than 500Pa. The progress of the polycondensation reaction is judged by the yield of EGDA and the mechanical stirring power of the reactor; the polycondensation reaction usually lasts for 0.5-4 hours to obtain the desired PET polymer.
[0008] The molar ratio of terephthalic acid to ethylene glycol diacetate is 1:1 to 1:2, preferably 1:1.2.
[0009] The catalyst includes: one or a combination of stannous oxalate, antimony trioxide, antimony acetate, antimony glycolate, boron trifluoride ethyl etherate, tetrabutyl titanate, bistrifluoromethanesulfonimide. Preferably, the catalyst is antimony trioxide, stannous oxalate or antimony acetate, and most preferably antimony acetate.
[0010] The system also includes a stabilizer, triethyl phosphoacetate, preferably added in an amount of 0.1 wt % based on the mass of terephthalic acid.
[0011] The mass ratio of the catalyst to terephthalic acid is 1:100000 to 1:100, preferably 1:0000 to 1:1000, and most preferably 1:2000.
[0012] The pressure in the reactor of the first stage transesterification reaction is 4-10 atm, and the temperature in the reactor is 240-280°C. Preferably, the pressure in the reactor is 8 atm, and the temperature is 260-280°C.
[0013] The temperature of the reactor for the second stage polycondensation is 270-290°C, and the vacuum degree is less than 500Pa. The preferred temperature is 280°C, and the vacuum degree is less than 200Pa.
[0014] The PET polymerization method of the present invention is a novel polymerization route using different polymerization raw materials (terephthalic acid and ethylene glycol diacetate), and the molecular weight of the obtained polymer exceeds 15,000. In the method, no undesired condensation mode (such as the formation of diethylene glycol fragments) will occur to affect the polymer properties; and because EG is not used, the tolerance to oxygen during the reaction process is stronger, and the produced PET will be more resistant to oxidation and yellowing. On the other hand, the boiling point of EGDA is lower than that of EG, so in theory EGDA is easier to leave the system, and the evaporated EGDA has no other impurities and can be directly used for the next polymerization. In addition, the method provides a new route and idea for the synthesis of PET. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The nuclear magnetic resonance hydrogen spectra of PET oligomers and polymers obtained according to the present invention in CF3COOD ( 1 1H NMR).
[0016] Figure 2 These are DSC images of PET obtained using the present invention (Example 6) and PET obtained using ethylene glycol (Example 10) as substrates.
[0017] Figure 3 It is the influence of different catalysts on the polymerization results. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0019] The present invention is a novel synthetic route for polyethylene terephthalate, the core technology of which is that ethylene glycol diacetate is used as one of the polymerization principles. During the depolymerization process, the structure of the polymer is characterized by nuclear magnetic resonance (NMR), the molecular weight of the polymer is determined by gel chromatography (GPC), and the thermal properties are characterized by differential scanning calorimetry (DSC).
[0020] Example 1-6: Effect of different catalysts on the molecular weight of polyethylene terephthalate
[0021] Terephthalic acid (100g), ethylene glycol diacetate (105g, 1.2eq) and catalyst (50mg, 0.05wt.%) were mixed in a 500mL titanium-lined polyester reactor. The air in the reactor was then replaced with nitrogen, and the pressure in the polyester reactor was finally maintained at 8atm. The transesterification reaction occurred at 260-280°C, and the pressure was controlled at around 8atm. The progress of the reaction was evaluated by the output of the by-product acetic acid, and the transesterification reaction was completed after about 4 hours. Subsequently, the polycondensation reaction began at 280°C and a high vacuum of less than 200Pa. The polycondensation reaction lasted for 3 hours to obtain the desired polymer. The number average molecular weight (Mn), weight average molecular weight (Mw) and polydispersity index (PDI) of the polymer are shown in Figure 3 The effects of different catalysts on polymerization results are shown in Figure 3 .
[0022] The experimental results show that antimony trioxide is the best polymerization catalyst. The product is not only slightly yellowish in color, but more importantly, the degree of polymerization exceeds 15,000, which meets the requirements of fiber-grade PET for the degree of polymerization. Especially after adding 0.1wt% of the stabilizer triethyl phosphoacetate, not only the color of PET is whiter, but also the molecular weight of PET is improved to a certain extent.
[0023] Example 7-9: Effect of the feed ratio of TPA and EGDA on the polymerization reaction
[0024] Terephthalic acid (100 g), different masses of ethylene glycol diacetate, antimony trioxide (50 mg, 0.05 wt.%) and triethyl phosphoacetate (100 mg, 0.1 wt.%) were mixed in a 500 mL titanium-lined polyester reactor. The air in the reactor was then replaced with nitrogen, and the polyester reactor pressure was finally maintained at 8 atm. The transesterification reaction occurred at 260-280 ° C, and the pressure was controlled at about 8 atm. The progress of the reaction was evaluated by the output of the by-product acetic acid, and the transesterification reaction was completed after about 4 hours. Subsequently, the polycondensation reaction began at 280 ° C and a high vacuum of less than 200 Pa. The polycondensation reaction lasted for 3 hours to obtain the desired polymer. The number average molecular weight (Mn), weight average molecular weight (Mw) and polydispersity index (PDI) of the polymer are shown in Table 1 below.
[0025] Table 1 Effect of feed ratio of TPA and EGDA on polymerization reaction
[0026]
[0027] The experimental results show that when the amount of EGDA is 1.02eq, the molecular weight of the PET polymer is not high due to the insufficient amount of EGDA. When the amount of EGDA is further increased to 1.5eq, the molecular weight of the PET polymer does not increase significantly. Therefore, only when the molar ratio of EGDA to TPA is 1.2, the polymerization effect of PET is the best.
[0028] Embodiment 10:
[0029] Terephthalic acid (100 g), ethylene glycol (75 g, 1.2 eq), antimony trioxide (50 mg, 0.05 wt.%) and triethyl phosphoacetate (100 mg, 0.1 wt.%) were mixed in a 500 mL titanium-lined polyester reactor. The air in the reactor was then replaced with nitrogen, and the polyester reactor pressure was finally maintained at 8 atm. The transesterification reaction occurred at 260-280 ° C, and the pressure was controlled at about 8 atm. The progress of the reaction was evaluated by the output of the by-product acetic acid, and the transesterification reaction was completed after about 4 hours. Subsequently, the polycondensation reaction began at 280 ° C and a high vacuum of less than 200 Pa. The polycondensation reaction lasted for 3 hours to obtain the desired polymer. The number average molecular weight of the resulting polymer: 37014, the weight average molecular weight: 67002, and the polydispersity coefficient: 1.81.
Claims
1. A method for synthesizing polyethylene terephthalate, characterized in that: Polyethylene terephthalate is obtained by polymerization of terephthalic acid and ethylene glycol diacetate as polymerization raw materials.
2. The synthesis method according to claim 1, characterized in that: Terephthalic acid, ethylene glycol diacetate and a catalyst are mixed in a polyester reactor, the air in the reactor is replaced by an inert gas, and finally a certain pressure is maintained in the polyester reactor, and then the temperature is increased. The first stage of the transesterification reaction occurs at 240-280°C. After the transesterification reaction is completed, the second stage of the polycondensation reaction occurs at 270-290°C. The polycondensation reaction time is 0.5-4 hours to obtain the desired PET polymer.
3. The synthesis method according to claim 2, characterized in that: The molar ratio of terephthalic acid to ethylene glycol diacetate is 1:1 to 1:
2.
4. The synthesis method according to claim 2, characterized in that: The catalyst is selected from one or a combination of stannous oxalate, antimony trioxide, antimony acetate, antimony glycolate, boron trifluoride etherate, tetrabutyl titanate, and bistrifluoromethanesulfonimide.
5. The synthesis method according to claim 4, characterized in that: The mass ratio of the catalyst to terephthalic acid is 1:100000 to 1:
100.
6. The synthesis method according to claim 2, characterized in that: The reaction system also includes triethyl phosphoacetate as a stabilizer.
7. The synthesis method according to claim 2, characterized in that: During the first stage of the transesterification reaction, the pressure in the reactor is controlled at 4-10 atm and the temperature in the reactor is 240-280°C.
8. The synthesis method according to claim 2, characterized in that: During the second stage of polycondensation reaction, the reactor temperature is 270-290°C and the vacuum degree is less than 500Pa.
Citation Information
Patent Citations
Production of esters of hydroxyethyl terephthalates
GB1364653A
Process of producing terephthalic acid reaction products
GB1387681A
New process for the manufacture of highly polymeric linear esters of terephthalic acid
GB590417A
Process of producing terephthalic acid reaction products
US3745182A