Preparation method of cross-linked high-temperature-resistant polyimide material
By using the cross-linking reaction of diamine monomers containing benzimidazole structure and aromatic cross-linking agent in deionized water solution, the problem of insufficient thermal stability of polyimide materials is solved, the glass transition temperature is increased, and it is suitable for for high-temperature flexible display materials.
Patent Information
- Application Number
- CN202410857707.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
AI Technical Summary
The glass transition temperature (Tg) of existing polyimide materials is generally around 300ºC, which cannot meet the requirements of the high-temperature production process of flexible displays. Moreover, the commonly used cross-linking agents have insufficient thermal stability and the cross-linking bonds contain secondary amine groups. Easy to degrade, affecting material performance.
The polyimide is prepared in one step using a diamine monomer and a dianhydride monomer containing a benzimidazole structure through an imidization catalyst, and is cross-linked with a cross-linking agent and an acid-binding agent in a deionized water solution under nitrogen protection to form The cross-linking bonds do not contain secondary amine groups, and aromatic cross-linking agents and deionized water are used to increase the degree of cross-linking.
The heat resistance of cross-linked polyimide is significantly improved, and the glass transition temperature (Tg) reaches above 400ºC, making it suitable for electronic packaging and circuit substrate materials.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a cross-linked high-temperature resistant polyimide. Background Art
[0002] Polyimide refers to a class of aromatic heterocyclic polymers containing an imide ring structure on the main chain, which are usually prepared by polycondensation of organic aromatic diamines and tetracarboxylic dianhydrides or derivatives. Polyimide contains a large number of symmetrical aromatic heterocyclic structures and polar groups, and the molecular chain has strong rigidity, order and strong interaction. Polyimide materials have high heat resistance, mechanical properties and dielectric properties, and are at the top of the material pyramid. They have been widely used in many cutting-edge high-tech fields such as microelectronics, aerospace, petrochemicals, membrane separation, etc.
[0003] Polyimide materials are the preferred materials for OLED flexible substrates due to their toughness, certain light transmittance and heat resistance. In the production process of flexible displays, the process temperature can reach up to 400°C or above. At the same time, flexible displays are very sensitive to dimensional changes caused by thermal and mechanical stresses, which puts forward new requirements for the heat resistance and high-temperature dimensional stability of flexible substrates. However, the glass transition temperature ( T g , that is, the upper limit temperature of long-term use) is generally around 300ºC. In order to meet the requirements of high-performance polyimide films in the high-temperature production process of flexible displays, it is urgent to develop films with higher thermal stability ( T g Polyimide material (above 400ºC).
[0004] Crosslinking between molecular chains is an effective way to improve the heat resistance of polyimide. The commonly used crosslinking strategy is to introduce monomers containing crosslinking sites and use crosslinkers to complete chemical crosslinking after polymerization. However, the crosslinkers currently used may have insufficient thermal stability, which may lead to degradation of the crosslinker during use, resulting in a decrease in material performance; or the generated crosslinked bonds contain groups with poor thermal stability such as secondary amines, which are prone to oxidation and other degradation reactions under high temperature conditions, affecting the actual performance of the material; there are problems such as poor solubility of inorganic acid binders in the solution during the crosslinking reaction process, resulting in a relatively low degree of crosslinking. How to select suitable crosslinkers and crosslinking reaction conditions through molecular structure design, while satisfying the requirement that sufficient crosslinking reactions occur and crosslinking sites are not easily degraded, is a key issue that needs to be solved in practical applications. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a cross-linked polyimide having a stable structure, good high temperature resistance and a high degree of cross-linking, wherein the key types of cross-linkable monomers, types of cross-linking agents, cross-linking reaction conditions, etc. are optimized to obtain a polyimide material with a higher glass transition temperature.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: A method for preparing a cross-linked high temperature resistant polyimide material comprises the following steps: (1) dissolving a diamine monomer containing benzimidazole, a dianhydride monomer and an imidization catalyst in a solvent A, and directly preparing a polyimide by one-step imidization using the imidization catalyst; (2) The polyimide is dissolved in a mixture of solvent B and deionized water, and a cross-linking agent and an acid-binding agent are added thereto. Under nitrogen protection, the mixture is further cross-linked to form a cross-linked polyimide.
[0007] Preferably, in step (1), the diamine monomer containing benzimidazole is any one of 2-(5-aminobenzimidazole-2-yl)benzene or 2-(3-aminophenyl)-5-aminobenzimidazole or 1,4-bis(4-aminophenyl)-5-aminobenzimidazole or 2,2'-bis(4-aminophenyl)-5,5'-bibenzimidazole or 1H,1'H-(2,2'-bibenzimidazole)-5,5'-diamine; the dianhydride monomer is pyromellitic acid dianhydride or 3,3',4,4' - any one of biphenyltetracarboxylic dianhydride or 3,3',4,4'-benzophenonetetracarboxylic dianhydride or 4,4'-(hexafluoroisopropyl) diphthalic anhydride or 3,3',4,4'-diphenyl ethertetracarboxylic dianhydride; the imidization catalyst is any one of isoquinoline or o-hydroxybenzoic acid or benzoic acid; solvent A is m-cresol or a mixture of m-cresol and any one of halogenated alkane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, sulfolane, and N-methylpyrrolidone.
[0008] Preferably, in step (1), the molar ratio of the benzimidazole-containing diamine monomer to the dianhydride monomer is 1:1, the mass ratio of the dianhydride monomer to the imidization catalyst and solvent A is 1:0.001-0.01:10-100, and the temperature of the polyimide polymerization reaction is 180-220°C and the time is 1-24h.
[0009] Preferably, in step (2), solvent B is a halogenated alkane or N,N-dimethylformamide or N,N-dimethylacetamide or dimethyl sulfoxide or cyclopentane or N-methylpyrrolidone or m-cresol, and in a mixed solution thereof with deionized water, the volume ratio of solvent B to deionized water is 99.5:0.5-98:2; the cross-linking agent is any one of trimesoyl chloride or terephthaloyl chloride or 4,4'-difluorobenzophenone or p-difluorobenzene; and the acid binding agent is any one of potassium carbonate or sodium carbonate or cesium carbonate.
[0010] Preferably, in step (2), the ratio of the mass of the polyimide, the total mass of solvent B and deionized water, the mass of the crosslinking agent, and the mass of the acid binding agent is 1:4-20:0.001-0.01:5-100, the temperature of the crosslinking reaction is 60-120° C., and the time of the crosslinking reaction is 1-24 hours.
[0011] Compared with the prior art, the present invention has the following beneficial effects: The diamine monomer containing a benzimidazole structure provided by the present invention utilizes the secondary amine in the benzimidazole structure as a cross-linking site. After cross-linking, the secondary amine group of the benzimidazole is converted into a tertiary amine structure. The generated cross-linking bonds no longer contain groups with poor thermal stability such as secondary amines, and no active hydrogen is present, so that the heat resistance of the cross-linking site is significantly improved.
[0012] In the technical solution of the present invention, the aromatic cross-linking agent selected through experiments is cross-linked with benzimidazole, and the aromatic structure can be retained after cross-linking, and groups with poor stability such as secondary amines will not be generated; the prepared cross-linked polyimide has more excellent heat resistance and can be used for electronic packaging materials or circuit substrate materials.
[0013] The technical solution of the present invention increases the solubility of the acid binding agent and the cross-linking degree of the product by adding deionized water as a cross-linking reaction solvent, so that the prepared cross-linked polyimide has better heat resistance. DETAILED DESCRIPTION
[0014] The following examples can enable those skilled in the art to more fully understand the present invention, but do not limit the present invention in any way. Example 1
[0015] 2,2′-bis(4-aminophenyl)-5,5′-bibenzimidazole and pyromellitic acid dianhydride are dissolved in m-cresol in a molar ratio of 1:1, and isoquinoline is added thereto, wherein the mass ratio of pyromellitic acid dianhydride to isoquinoline and m-cresol is 1:0.01:100, and imidization reaction occurs under nitrogen protection, and the reaction temperature is controlled at 220°C. After reacting for 1 hour, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide; A mixed solution of polyimide, N,N-dimethylformamide and deionized water (volume ratio 98:2), p-difluorobenzene and potassium carbonate in a mass ratio of 1:20:0.01:5 were mixed, dissolved and cross-linked, and the cross-linking reaction temperature was controlled at 60°C. After reacting for 12 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a cross-linked high-temperature resistant polyimide material, named 1# cross-linked polyimide. Example 2
[0016] 2-(5-aminobenzimidazol-2-yl)benzene and 3,3',4,4'-biphenyltetracarboxylic dianhydride are dissolved in m-cresol at a molar ratio of 1:1, and isoquinoline is added thereto, wherein the mass ratio of dianhydride monomer to isoquinoline and m-cresol is 1:0.001:10, and imidization reaction occurs under nitrogen protection, and the reaction temperature is controlled at 180°C. After reacting for 24 hours, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide; A mixed solution of polyimide, N,N-dimethylformamide and deionized water (volume ratio of 99.5:0.5), trimesoyl chloride and potassium carbonate are mixed and dissolved in a mass ratio of 1:4:0.001:100 to cause a cross-linking reaction. The cross-linking reaction temperature is controlled at 60°C. After reacting for 24 hours, the reaction solution is poured into ethanol to form a precipitate. The precipitate is filtered, washed and dried to obtain a cross-linked high-temperature resistant polyimide material, named 2# cross-linked polyimide. Example 3
[0017] 2-(3-aminophenyl)-5-aminobenzimidazole and 3,3',4,4'-benzophenone tetracarboxylic dianhydride are dissolved in a mixed solution of m-cresol and dimethyl sulfoxide at a molar ratio of 1:1, wherein the volume ratio of m-cresol to dimethyl sulfoxide is 3:2, and o-hydroxybenzoic acid is added thereto, wherein the mass ratio of the dianhydride monomer to the o-hydroxybenzoic acid and the m-cresol / dimethyl sulfoxide mixed solvent is 1:0.005:50, and an imidization reaction occurs under nitrogen protection, and the reaction temperature is controlled at 200°C. After reacting for 12 hours, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide. In this step, the solvent is a mixed solution of m-cresol and any one of halogenated alkanes, N,N-dimethylformamide, N,N-dimethylacetamide, cyclopentane, and N-methylpyrrolidone, mixed at a volume ratio of 5:1-5, which can also achieve the purpose of the present invention.
[0018] The mixed solution of polyimide, N-methylpyrrolidone and deionized water (volume ratio of 99:1), terephthaloyl chloride and sodium carbonate were mixed and dissolved in a mass ratio of 1:5:0.005:50 to cause a cross-linking reaction. The cross-linking reaction temperature was controlled at 100°C. After reacting for 12 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a cross-linked high-temperature resistant polyimide material, named 3# cross-linked polyimide. Example 4
[0019] 1,4-bis(4-aminophenyl)-5-aminobenzimidazole and 4,4'-(hexafluoroisopropyl) diphthalic anhydride are dissolved in m-cresol at a molar ratio of 1:1, and benzoic acid is added thereto, wherein the mass ratio of the dianhydride monomer to benzoic acid and m-cresol is 1:0.002:80, and imidization reaction occurs under nitrogen protection, and the reaction temperature is controlled at 180°C. After reacting for 18 hours, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide; A mixed solution of polyimide, meta-cresol and deionized water (volume ratio of 99.5:0.5), 4,4'-difluorobenzophenone and sodium carbonate were mixed and dissolved in a mass ratio of 1:7:0.01:25 to cause a cross-linking reaction. The cross-linking reaction temperature was controlled at 120°C. After reacting for 5 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a cross-linked high-temperature resistant polyimide material, named 4# cross-linked polyimide. Example 5
[0020] 1H,1'H-(2,2'-bibenzimidazole)-5,5'-diamine and 3,3',4,4'-diphenylether tetracarboxylic dianhydride are dissolved in a mixed solution of m-cresol and sulfolane at a molar ratio of 1:1, wherein the volume ratio of m-cresol to sulfolane is 1:1, and isoquinoline is added thereto, wherein the mass ratio of the dianhydride monomer to the isoquinoline and m-cresol / sulfolane mixed solution is 1:0.007:50, and imidization reaction occurs under nitrogen protection, the reaction temperature is controlled at 200°C, and after reacting for 10 hours, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide; in this step, the solvent is a mixed solution of m-cresol and any one of halogenated alkanes, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone, mixed at a volume ratio of 5:1-5, which can also achieve the purpose of the present invention.
[0021] A mixed solution of polyimide, N-methylpyrrolidone and deionized water (volume ratio of 98:2), p-difluorobenzene and potassium carbonate in a mass ratio of 1:10:0.002:10 were mixed, dissolved and cross-linked, and the cross-linking reaction temperature was controlled at 100°C. After reacting for 12 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a cross-linked high-temperature resistant polyimide material, named 5# cross-linked polyimide.
[0022] Comparative Example 1 (Preparation of polyimide without cross-linking structure) 2,2′-bis(4-aminophenyl)-5,5′-bibenzimidazole and pyromellitic anhydride were dissolved in m-cresol at a molar ratio of 1:1, and isoquinoline was added thereto, wherein the mass ratio of pyromellitic anhydride to isoquinoline and m-cresol was 1:0.01:100. Under nitrogen protection, imidization reaction occurred, and the reaction temperature was controlled at 220°C. After reacting for 1 hour, the reaction solution was poured into ethanol to obtain a precipitate, and the precipitate was filtered, washed, and dried to obtain a polyimide, which was named 1# comparative polyimide.
[0023] Comparative Example 2 (Preparation of a cross-linked polyimide material using a diamine monomer not containing a benzimidazole structure) Dissolve diamine 4,4′-diaminodiphenyl ether without a benzimidazole structure and pyromellitic dianhydride in m-cresol at a molar ratio of 1:1, add isoquinoline thereto, wherein the mass ratio of dianhydride monomer to isoquinoline and m-cresol is 1:0.007:50, and carry out imidization reaction under nitrogen protection, control the reaction temperature at 200° C., react for 10 hours, pour the reaction solution into ethanol to obtain a precipitate, filter, wash and dry the precipitate to obtain a polyimide; Polyimide, N-methylpyrrolidone, p-difluorobenzene and potassium carbonate were mixed and dissolved in a mass ratio of 1:10:0.002:10 to produce a cross-linking reaction. The cross-linking reaction temperature was controlled at 120°C. After reacting for 12 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a cross-linked polyimide material, which was named 2# comparative polyimide.
[0024] Comparative Example 3 (Preparation of cross-linked polyimide material using non-aromatic cross-linking agent) 1H,1'H-(2,2'-bibenzimidazole)-5,5'-diamine and pyromellitic dianhydride are dissolved in m-cresol at a molar ratio of 1:1, and isoquinoline is added thereto, wherein the mass ratio of dianhydride monomer to isoquinoline and m-cresol is 1:0.007:50, and imidization reaction occurs under nitrogen protection, and the reaction temperature is controlled at 200°C. After reacting for 10 hours, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide; Polyimide, N-methylpyrrolidone, triglycidyl isocyanurate and potassium carbonate were mixed and dissolved in a mass ratio of 1:10:0.002:10 to produce a cross-linking reaction. The cross-linking reaction temperature was controlled at 100°C. After reacting for 12 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a cross-linked polyimide material, which was named 3# comparative polyimide.
[0025] Comparative Example 4 (Partially cross-linked polyimide material in which deionized water is not added as a cross-linking reaction solvent) 1H,1'H-(2,2'-bibenzimidazole)-5,5'-diamine and pyromellitic dianhydride are dissolved in m-cresol at a molar ratio of 1:1, and isoquinoline is added thereto, wherein the mass ratio of dianhydride monomer to isoquinoline and m-cresol is 1:0.007:50, and imidization reaction occurs under nitrogen protection, and the reaction temperature is controlled at 200°C. After reacting for 10 hours, the reaction solution is poured into ethanol to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a polyimide; Polyimide, N-methylpyrrolidone, p-difluorobenzene and potassium carbonate were mixed and dissolved in a mass ratio of 1:10:0.002:10 to produce a cross-linking reaction. The cross-linking reaction temperature was controlled at 100°C. After reacting for 12 hours, the reaction solution was poured into ethanol to form a precipitate. The precipitate was filtered, washed and dried to obtain a partially cross-linked polyimide material, named 4# comparative polyimide.
[0026] The glass transition temperatures of the polyimides in Examples 1-5 and Comparative Examples 1-4 are tabulated and analyzed. As shown in Table 1, compared with Comparative Example 1, the examples all have crosslinked structures after crosslinking reactions. T g are higher than those in Comparative Example 1, indicating that the cross-linking process can significantly improve the T g .
[0027] Compared with Comparative Example 2, the diamine monomer selected in Comparative Example 2 does not contain a benzimidazole structure. Even if the cross-linking reaction step is performed, no effective cross-linking reaction occurs. T g Relatively low, the embodiment T g All of them are higher than Comparative Example 2. This indicates that the selected diamine monomer structure containing a benzimidazole structure is helpful to improve the heat resistance of the material.
[0028] Compared with Comparative Example 3, the crosslinking agent selected in Comparative Example 3 is a non-aromatic crosslinking agent, which has slightly poor thermal stability and large steric hindrance, which is not conducive to the material T g Therefore, the embodiment of the present invention T gAll of them are higher than Comparative Example 3. This indicates that the use of a cross-linking agent containing aromatic substances itself is helpful to improve the heat resistance of the material.
[0029] Compared with Comparative Example 4, although an aromatic crosslinking agent was selected in Comparative Example 4, the solvent for the crosslinking reaction did not contain deionized water, and the acid-binding agent potassium carbonate was basically insoluble in the reaction system. The reaction with the generated byproduct hydrogen fluoride was a solid-liquid reaction, and the reaction rate was low. The degree of promotion of the crosslinking reaction was low, resulting in the final generated polymer T g The improvement is limited. This shows that adding some deionized water during the cross-linking reaction can improve the heat resistance of the material.
[0030]
[0031] Comprehensive analysis shows that the present invention selects a diamine monomer containing a benzimidazole structure, and utilizes the secondary amine in the benzimidazole structure as a cross-linking site. After cross-linking, the secondary amine group of the benzimidazole becomes a tertiary amine structure without active hydrogen, and the heat resistance of the cross-linking site is significantly improved; deionized water is added to the reaction solution during the cross-linking reaction, which increases the solubility of the acid binding agent in the reaction solution, increases the degree of cross-linking reaction, and further increases the heat resistance of the material.
[0032] The aromatic crosslinking agent selected in the present invention can form an aromatic structure after crosslinking with benzimidazole, and has excellent thermal stability; by adding deionized water to the crosslinking reaction system, the degree of crosslinking reaction is further increased, and finally the prepared crosslinked polyimide has better heat resistance and higher glass transition temperature ( T g ), that is, it has higher heat resistance and can be used for electronic packaging materials or circuit substrate materials.
Claims
1. A method for preparing a cross-linked high temperature resistant polyimide material, characterized in that: The following steps are involved: (1) dissolving a diamine monomer containing benzimidazole, a dianhydride monomer and an imidization catalyst in a solvent A, and directly preparing a polyimide by a one-step imidization using the imidization catalyst; (2) The polyimide is dissolved in a mixed solution of solvent B and deionized water, and a crosslinking agent and an acid binding agent are added thereto. Under nitrogen protection, a crosslinking reaction occurs to obtain a crosslinked polyimide.
2. The method for preparing the cross-linked high temperature resistant polyimide according to claim 1, characterized in that: In the step (1), the diamine monomer containing benzimidazole is any one of 2-(5-aminobenzimidazole-2-yl)benzene or 2-(3-aminophenyl)-5-aminobenzimidazole or 1,4-bis(4-aminophenyl)-5-aminobenzimidazole or 2,2'-bis(4-aminophenyl)-5,5'-bibenzimidazole or 1H,1'H-(2,2'-bibenzimidazole)-5,5'-diamine; the dianhydride monomer is pyromellitic dianhydride or 3,3',4,4'-bibenzimidazole. Any one of benzenetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-(hexafluoroisopropyl) diphthalic anhydride, or 3,3',4,4'-diphenyl ethertetracarboxylic dianhydride; the imidization catalyst is any one of isoquinoline, o-hydroxybenzoic acid, or benzoic acid; solvent A is m-cresol or a mixture of m-cresol and any one of halogenated alkane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, sulfolane, or N-methylpyrrolidone.
3. The method for preparing the cross-linked high temperature resistant polyimide according to claim 1, characterized in that: In the step (1), the molar ratio of the benzimidazole-containing diamine monomer to the dianhydride monomer is 1:1, the mass ratio of the dianhydride monomer to the imidization catalyst and the solvent A is 1:0.001-0.01:10-100, and the reaction temperature for preparing the polyimide is 180-220°C and the reaction time is 1-24h.
4. The method for preparing the cross-linked high temperature resistant polyimide according to claim 1, characterized in that: In the step (2), solvent B is a halogenated alkane or N,N-dimethylformamide or N,N-dimethylacetamide or dimethyl sulfoxide or cyclopentane or N-methylpyrrolidone or m-cresol, and in a mixed solution thereof with deionized water, the volume ratio of solvent B to deionized water is 99.5:5-98:2; the cross-linking agent is any one of trimesoyl chloride or terephthaloyl chloride or 4,4'-difluorobenzophenone or p-difluorobenzene; and the acid binding agent is any one of potassium carbonate or sodium carbonate or cesium carbonate.
5. The method for preparing the cross-linked high temperature resistant polyimide according to claim 1, characterized in that: In step (2), the mass ratio of the total mass of the polyimide, solvent B and deionized water, the crosslinking agent and the acid binding agent is 1:4-20:0.001-0.01:5-100, the temperature of the crosslinking reaction is 60-120° C., and the time of the crosslinking reaction is 1-24 hours.