Silicone compositions for low temperature applications

Through the method of low-temperature hydrolysis of silanol precursors and specific catalysts, silicone materials with low glass transition temperature and high molecular weight are synthesized, which solves the problem of silicone materials losing elasticity in extreme low-temperature environments and achieves safe and efficient Siloxane synthesis for extreme applications such as space exploration.

CN118772410APending Publication Date: 2024-10-15VENTURI LAB AG
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410399382.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2024-04-03
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing silicone materials lose elasticity and mechanical properties in extremely low-temperature environments and cannot meet the needs of extreme low-temperature applications such as space exploration. Moreover, traditional synthesis methods have problems such as high-temperature reactions, excessive gas products, and explosion risks.

Method used

Poly(dimethyl-co-) with low glass transition temperature and high molecular weight was synthesized by low-temperature hydrolysis of silanol precursor, using indium trifluoromethanesulfonate and perfluoroborane catalyst, and Lewis acid-induced polycondensation reaction. diethyl)siloxane or poly(methylhydrogen-co-diethyl)siloxane, reduce cyclic siloxane by-products, and develop new cross-linkers with excellent compatibility with PDIES.

Benefits of technology

It achieves the synthesis of high molecular weight siloxane materials at low temperatures, avoids the problems of high temperature reactions and excessive gas products, improves the mechanical properties and safety of the materials, and is suitable for extreme low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004775117070000041
    Figure BDA0004775117070000041
  • Figure BDA0004775117070000042
    Figure BDA0004775117070000042
  • Figure BDA0004775117070000051
    Figure BDA0004775117070000051
Patent Text Reader

Abstract

The invention relates to a method for producing methyl and ethyl-containing polysiloxanes, comprising the following steps: a) hydrolysis reaction of a silanol precursor, b) polycondensation induced by a Lewis acid by adding a trifluoromethanesulfonate catalyst followed by adding a perfluoroborane catalyst, the chain of the silanol-terminated siloxane oligomer obtained in step a) is increased by adding a silane to the silane-terminated siloxane oligomer obtained in step a). The invention also relates to a poly (dimethyl-co-diethyl) siloxane of formula (IIIa), a poly (methyl hydrogen-co-diethyl) siloxane of formula (IIIb), a composition for preparing a silicone rubber comprising said polymer, a silicone rubber obtainable by curing the composition and the use of the silicone rubber in the aerospace industry. The invention also relates to poly (dimethyl-co-diethyl) siloxanes of formula V and their use in the aerospace industry.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to European patent application serial number EP23167067.0 filed on April 6, 2023, the entire contents of which are incorporated herein by reference.

[0002] The field of the invention is reinforced silicone rubber and silicone oil compositions capable of withstanding the extremely low temperatures required for aerospace applications.

[0003] Silicone is an organosilicon polymer with a siloxane structure, characterized in that the silicon atom is connected to an alkyl group such as an ethyl or methyl group, a trifluoromethyl group, an aryl group, and other functional groups. Silicone rubber compositions derived from poly(dimethylsiloxane) (commonly referred to as PDMS) are known to withstand temperatures as low as -60°C. However, many space applications such as space exploration missions require silicone materials to withstand temperatures far below -100°C, as well as a yield tensile strength of >3MPa and an elongation at break of more than 300%.

[0004] Poly(diethylsiloxane) (PDIES) is the only polymer material with a glass transition temperature of -142°C. However, pure PDIES undergoes multiple crystallization / melting transitions from -142°C to 0°C, making it unsuitable for such applications. Crystallization of silicon is usually accompanied by its hardening, brittleness and loss of elasticity, which may lead to degradation of mechanical properties or even catastrophic loss of objects used in vehicle applications (such as space rovers). It is known from the prior art that the addition of small amounts of phenyl, biphenyl or diethyl (less than 10 mol%) to poly(dimethylsiloxane) can prevent cold-induced crystallization of dimethylpolysiloxane copolymers. In fact, the vast majority of commercially available space silicones currently sold on the market (Momentive, Elkem, Nusil, Dow Corning, IOTA Corporation Ltd, etc.) belong to the family of poly(biphenyl-co-dimethylsiloxane) or poly(methylphenyl-co-dimethylsiloxane). Interestingly, in such copolymers, increasing the content of biphenyl or methyl-phenyl to above 10 mol% makes the glass transition temperature even higher and thus limits the extremely low temperature applications (down to -150°C). For example, the glass transition temperature Tg = -115°C of RTV 560, RTV 566, RTV 567 (methyl-phenyl silicones) sold by Momentive makes such materials unsuitable for South Pole missions on the Moon. It is important to note that cold crystallization of RTV 566 under 25% strain and long-term waiting (60 hours) at -80°C induces an increase in its elastic modulus from 5 MPa to 240 MPa, which may be the main reason for its mechanical failure and telescope misalignment.

[0005] Currently, there are no commercially available silicones with relatively high tensile strength (i.e., above 4 MPa), elongation at break above 100%, and low temperature resistance below -120° C. The only commercially available silicone is sold by Gelest (EDV-2022), which contains 18-22 mol% poly(diethylsiloxane) and 78-82 mol% poly(dimethylsiloxane), Tg=-131° C. However, this material has a relatively low molecular weight (10000-12000 g / mol), and it may contain cyclic siloxane oligomers that make it brittle, and is therefore not suitable for aerospace applications.

[0006] The traditional method of silicone synthesis relies on the hydrolysis of dimethyldichlorosilane, which hydrolyzes to produce disilanol H[O-Si(CH3)2] n -OH, hydrochloric acid and a variable amount of cyclic siloxane. The hydrochloric acid then acts as a catalyst for the condensation of disilanols into polydimethylsiloxane. From this, various methods can be used to polymerize silanol-terminated silicones, depending on the desired properties of the final product.

[0007] US4960850A describes the polycondensation of polydiorganosiloxane oligomers having silanol end groups in a closed reaction zone in the presence of a catalytically effective amount of trifluoromethylsulfonic acid at a temperature of 20°C to 160°C, while continuously removing water in the polycondensation using a vacuum, and terminating the polycondensation reaction by adding a catalyst-neutralizing amount of a cyclopolydiorganosilazane or a polydiorganosilazane having diorganoaminosilyl end groups to the reaction medium. However, trifluoromethylsulfonic acid has a boiling point of 162°C and can be distilled out while removing water under high vacuum.

[0008] Silicones with tailored molecular weights can be obtained in a highly controlled manner by ring-opening polymerization (ROP) of cyclic siloxanes, which also represents the main route in industry. In the case of polymerizing a single cyclic siloxane, the above method is relatively simple. However, when trying to copolymerize two cyclic siloxanes, such as copolymerizing decamethylcyclosiloxane (D5Me10) with hexaethylcyclosiloxane (D3Et6) to prepare 1:1 poly(dimethyl-co-diethyl)siloxane, the copolymerization process becomes difficult to control, the latter originating from the different strains on the monomer molecules and the different ring-opening kinetics of D3Et6 and D5Me10. Ring opening requires relatively high reaction temperatures of 95°C-160°C, suitable anionic initiators, end-capping agents, additives, pressure-treated reactors, etc. Silicones usually undergo a certain degree of decomposition (back biting), producing various amounts (or varying amounts) of cyclic siloxanes, which may be difficult to remove from high-viscosity silicones. Furthermore, hexaethylcyclosiloxane is known to polymerize preferentially with itself, forming brittle domains in the crosslinked rubber, which leads to poor mechanical properties of the obtained material.

[0009] Another method for synthesizing polysiloxanes using monomeric silane precursors is to rely on the polycondensation of silane monomers or oligomers in the presence of perfluoroarylborane catalysts such as B(C6F5)3. (Michael A. Brooks, J Brande, F. Ganachaud, New Synthetic Strategies for Structured Silicones Using B(C6F5)3. Adv. Polym. Sci. 2011, 235, 161-183). This method is called the Piers–Rubinsztajn reaction, and one of its advantages over ROP (which relies on cyclic monomers) is that it can be carried out at room temperature and produces much less cyclic products than high-temperature ROP synthesis. However, the main disadvantage of this method is that it can be used to synthesize small amounts of silicones (millimolar amounts), but it is unlikely to be used to synthesize kilogram amounts of dimethyl-co-diethyl (1:1) polysiloxanes. This is due to the fact that such reactions are extremely exothermic and generate large amounts of gaseous products (typically more than 100 liters of H2, CH4 or CH3-CH3 per kg of silicone). Obviously, this is associated with a serious explosion hazard when attempting to scale up the reaction. Furthermore, another disadvantage of using the Piers–Rubinsztajn reaction is that the borane catalyst must be dissolved in a solvent such as toluene (heptane causes it to precipitate) as water can cause catalyst degradation. During solvent-free silicone synthesis, the viscosity of the polymer is fairly straightforward as it can be checked at any time visually or by using a viscometer, however, in organic solvents such as toluene, it may be difficult to monitor the progress of the reaction. Furthermore, depending on the silane precursor structure (i.e. -OH, -OCH3 or -OCH2CH3), the reaction temperature must be elevated to polymerize the monomers. For example, the reaction of dimethoxydimethylsilane with the -OCH3 group of diethylsilane proceeds at 22°C-23°C, while 70°C is required to convert -OCH2CH3 to ethane in the presence of B(C6F5)3.

[0010] It is known from the prior art that the rate of hydrolysis of silanes depends on their electronic structure, the solvent used, the presence / absence of a catalyst and the reaction temperature. For example, while the hydrolysis of dichlorodimethylsilane in water occurs even at temperatures close to zero degrees, diethoxydimethylsilane is stable at 25° C. and its hydrolysis requires temperatures above 50° C. and ultimately requires the presence of a suitable acid or base catalyst.

[0011] The applicant has found that the low temperature (1°C-7°C) hydrolysis method of diethyl / dimethyl / ethylmethylchlorosilane can reproducibly obtain silanol-terminated poly(dimethyl-co-diethyl)siloxane or polymethylethylsiloxane with an average molecular weight of Mw-1000 (viscosity 33mPa.s-36mPa.s). In the presence of a suitable Lewis acid catalyst, it can be conveniently polymerized into high molecular weight PDIES or PEMS (Mw-50000-100000) with very low glass transition temperature and no crystallization / melting transition at low temperature. The method results in a relatively fast (within minutes) viscosity increase without the need for high reaction temperatures (above 100°C) and with minimal amounts of cyclic silicone by-products (parts per million). The PDIES / PEMS synthesis method of the present invention solves the problem of the formation of large amounts of gaseous products (H2, methane or ethane) experienced in the Piers–Rubinsztajn reaction, thereby limiting the high exothermicity and explosion hazard as discussed above.

[0012] Furthermore, another issue to be addressed is the compatibility of the crosslinker with vinyl terminated PDIES. Typically, crosslinking of phenyl silicones requires a phenyl containing crosslinker because phase separation and increased foaming occur when conventional methylhydrogen-(PHMS) or dimethyl-co-methylhydrogen polysiloxane crosslinkers are used. The applicants have noticed a similar phenomenon with the use of dimethyl-co-diethyl polysiloxane. When vacuum was applied to the PDIES / PHMS mixture in the absence or presence of silica, extensive foaming was observed. In order to address this crosslinker / diethyl silicone incompatibility issue, the applicants have synthesized a new -methylhydrogen-co-diethyl-siloxane crosslinker with excellent compatibility with PDIES.

[0013] Therefore, the present invention relates to a method for preparing a polysiloxane containing methyl and ethyl groups, the method comprising the following steps:

[0014] a) hydrolysis reaction of silanol precursor;

[0015] b) chain extension of the silanol-terminated siloxane oligomer obtained in step a) by Lewis acid-induced polycondensation by addition of a triflate catalyst, in particular indium(III) triflate, followed by addition of a perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane.

[0016] Advantageously, the methyl and ethyl containing polysiloxanes are selected from the group consisting of:

[0017] Poly(dimethyl-co-diethyl)siloxane or poly(methyl hydrogen-co-diethyl)siloxane represented by the following formula (I):

[0018]

[0019] Where A represents a methyl group or a hydrogen atom,

[0020] m and n represent the molar percentages of the repeating units –O-Si(Me)(A) and –O-Si(Et2), respectively.

[0021] m = 0.5-0.8, n = 0.2-0.5, and m + n = 1,

[0022] p represents the number of the two repeating units so as to obtain a weight average molecular weight in the range of 20000 g / mol to 150000 g / mol when A represents a methyl group and in the range of 300 g / mol to 3500 g / mol when A represents a hydrogen atom,

[0023] and,

[0024] Poly(ethylmethylsiloxane) represented by the following formula (II):

[0025]

[0026] Where q represents the number of repeating units.

[0027] More advantageously, the silanol precursor of step a) can be selected from (R1)2ethylmethylsilane, a mixture of (R1)2dimethylsilane and (R1)2diethylsilane, a mixture of (R1)2methylsilane and (R1)2diethylsilane, wherein R1 represents a chlorine atom, a (C1-C6)alkoxy group (advantageously a methoxy group or an ethoxy group), an acetoxy group or an oxime group, advantageously R1 represents a chlorine atom, a methoxy group or an ethoxy group, more advantageously R1 represents a chlorine atom.

[0028] In the chemical formulas involved in the present invention, Me is a methyl group, and Et is an ethyl group.

[0029] In terms of the present invention, the terms “included between x and y”, “in the range of xy”, “=xy”, “from x to y” are intended to mean including the limit values ​​x and y of the range.

[0030] For the purposes of the invention, the term "(C1-C6)alkoxy" is intended to mean any straight-chain or branched saturated alkoxy group having 1 to 6 carbon atoms, in particular the groups OCH3 (methoxy) and OCH2CH3 (ethoxy).

[0031] Therefore, the method according to the invention is used to prepare polysiloxanes containing methyl and ethyl groups, advantageously poly(dimethyl-co-diethyl)siloxanes or poly(methylhydrogen-co-diethyl)siloxanes described by the following formula (I):

[0032]

[0033] Where A represents a methyl group or a hydrogen atom,

[0034] m and n represent the molar percentages of the repeating units –O-Si(Me)(A) and –O-Si(Et2), respectively, where

[0035] m = 0.5-0.8, n = 0.2-0.5, and m + n = 1,

[0036] p represents the number of both repeating units so as to obtain a weight average molecular weight in the range of 20000 g / mol to 150000 g / mol when A represents a methyl group and in the range of 300 g / mol to 3500 g / mol when A represents a hydrogen atom. Viscometry (according to standard ASTM E3116-18 of January 25, 2018), 1H NMR and FTIR can be used to measure the weight average molecular weight of the polymer.

[0037] Advantageously, m=0.5-0.7, and n=0.3-0.5, wherein m+n=1, more advantageously, m=0.5-0.6, and n=0.4-0.5, wherein m+n=1, further advantageously, m=n=0.5.

[0038] In particular, the poly(dimethyl-co-diethyl)siloxane according to the invention has the following formula Ia:

[0039]

[0040] wherein m, n and p are as defined above.

[0041] Advantageously, the poly(dimethyl-co-diethyl)siloxane of formula Ia according to the invention has a weight average molecular weight of 20,000 to 150,000 g / mol, more advantageously 30,000 to 100,000 g / mol, still more advantageously 40,000 to 80,000 g / mol, in particular 45,000 to 60,000 g / mol, measured in particular using the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0042] In particular, the poly(methylhydrogen-co-diethyl)siloxane according to the present invention has the following formula Ib:

[0043]

[0044] wherein m, n and p are as defined above.

[0045] Advantageously, the poly(methylhydrogen-co-diethyl)siloxane of formula Ib according to the invention has a weight average molecular weight of 300 to 3500 g / mol, more advantageously 500 to 3000 g / mol, still more advantageously 1000 to 2000 g / mol, measured in particular using the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0046] The process according to the invention is also advantageously used for preparing poly(ethylmethylsiloxane) represented by the following formula (II):

[0047]

[0048] Where q represents the number of repeating units.

[0049] Advantageously, the poly(ethylmethylsiloxane) according to the invention has a weight average molecular weight ranging from 1000 g / mol to 2 000 000 g / mol, measured in particular using the viscometry method according to standard ASTM E3116-18 of 25 January 2018.

[0050] Step a) of the process according to the invention consists in the hydrolysis reaction of a silanol precursor.

[0051] Advantageously, the silanol precursor can be selected from (R1)2ethylmethylsilane, a mixture of (R1)2dimethylsilane and (R1)2diethylsilane, and a mixture of (R1)2methylsilane and (R1)2diethylsilane, wherein R1 represents a chlorine atom, a (C1-C6)alkoxy group (advantageously methoxy or ethoxy), an acetoxy group or an oxime group, advantageously R1 represents a chlorine atom, a methoxy group or an ethoxy group, more advantageously R1 represents a chlorine atom.

[0052] Thus, advantageously, the silanol precursors are chlorinated or ethoxylated silanol precursors, in particular chlorinated silanol precursors. More advantageously, they are selected from dichloroethylmethylsilane, diethoxyethylmethylsilane, a mixture of dichlorodimethylsilane and dichlorodiethylsilane, a mixture of dichloromethylsilane and dichlorodiethylsilane, a mixture of diethoxydimethylsilane and diethoxydiethylsilane, and a mixture of diethoxymethylsilane and diethoxydiethylsilane, more advantageously from dichloroethylmethylsilane, a mixture of dichlorodimethylsilane and dichlorodiethylsilane, and a mixture of dichloromethylsilane and dichlorodiethylsilane.

[0053] The product obtained after step a) is an oligomer of siloxane containing methyl and ethyl groups, in particular an oligomer of (dimethyl-co-diethyl)siloxane, or an oligomer of (methylhydrogen-co-diethyl)siloxane, or an oligomer of ethylmethylsiloxane. Advantageously, when A is methyl, these oligomers have a weight average molecular weight of 500 g / mol to 3000 g / mol, more advantageously 1000 g / mol to 3000 g / mol, measured using the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0054] Possible reaction schemes (Scheme 1 and Scheme 2) of step a) are as follows:

[0055]

[0056] wherein A, m and n are as defined above, and R1 represents a chlorine atom, a C1-C6 alkoxy group (particularly a methoxy or ethoxy group), an acetoxy group or an oxime group, advantageously R1 represents a chlorine atom, a methoxy group or an ethoxy group, more advantageously R1 represents a chlorine atom.

[0057] In an advantageous embodiment, step a) is performed at a temperature ranging from 0°C to 40°C, more advantageously from 5°C to 35°C.

[0058] In an advantageous manner, the reaction is first carried out at a temperature of 0°C to 7°C, advantageously 5°C to 7°C, and then the temperature is raised to a range of 30°C-40°C, advantageously 30°C-35°C.

[0059] More advantageously, the reaction is carried out under stirring, still more advantageously by adding an aqueous solution of the silanol precursor, in particular dropwise, more advantageously at a rate of 1 to 5 drops / second, in particular 3 drops / second.

[0060] In an advantageous embodiment, step a) lasts from 1 hour to 2 hours.

[0061] In an advantageous embodiment, the water molar concentration (w) is higher than the molar concentration of the two silanol precursors (a+b): w>a+b.

[0062] In a further embodiment, prior to step b) for the process according to the invention, the oligomers obtained in step a) are separated from the aqueous phase obtained after carrying out step a), advantageously by extraction with heptane, wherein the aqueous phase contains HR1, in particular HCl.

[0063] Step b) of the process according to the invention consists in extending the chain of the silanol-terminated siloxane oligomer obtained in step a), which can advantageously be a poly(dimethyl-co-diethyl)siloxane oligomer, or a poly(methylhydrogen-co-diethyl)siloxane oligomer, or an ethylmethylsiloxane oligomer, by adding a triflate catalyst and then a perfluoroborane catalyst, by means of a Lewis acid-induced polycondensation. Thus, advantageously, the polymer obtained after step b) is a polymer of formula I or II as detailed above.

[0064] Advantageously, the triflate catalyst is selected from indium(III) triflate, bismuth(III) triflate, aluminum(III) triflate and mixtures thereof, more advantageously indium(III) triflate.

[0065] Advantageously, the perfluoroborane catalyst is tris(pentafluorophenyl)borane.

[0066] The reaction schemes (Scheme 3 and Scheme 4) of step b) using indium(III) trifluoromethanesulfonate and tris(pentafluorophenyl)borane catalyst are as follows:

[0067]

[0068] wherein A, m, n and p are as defined above.

[0069]

[0070] where q is as defined above.

[0071] The polymers of formula (I) are alternating copolymers.

[0072] The polymer of formula (II) is a homopolymer.

[0073] Advantageously, step (b) is carried out at room temperature (20°C-25°C).

[0074] In an advantageous embodiment:

[0075] The triflate catalyst, in particular indium(III) triflate, is first added under stirring (step b1) and the reaction is then allowed to proceed without any stirring, advantageously for at least 1 hour to 12 hours.

[0076] A perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane, is then added with stirring (step b2) and the reaction is then allowed to proceed without any stirring, advantageously for at least 1 hour to 12 hours.

[0077] Advantageously, step (b) is carried out in bulk, without any solvent.

[0078] In an advantageous embodiment, the triflate catalyst, in particular indium(III) triflate, is present in an amount of 0.1 mg to 1 mg per gram of oligomer.

[0079] In another advantageous embodiment, the perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane, is present in an amount of 0.1 mg to 1 mg per gram of oligomer.

[0080] In a specific embodiment, step b) is carried out under an inert atmosphere, advantageously under a nitrogen atmosphere.

[0081] The process according to the invention may comprise a step c1) of adding vinyl end groups by reacting the polymer obtained in step b) with vinyldimethylmethoxysilane or vinyl-1,1,3,3-tetramethyldisiloxane at a temperature ranging from 20° C. to 60° C. and in the presence of a Lewis acid catalyst such as indium(III) trifluoromethanesulfonate in the absence of any solvent, or B(C6F5)3 in toluene as solvent, or B(C6F5)3 in the absence of any solvent, advantageously in order to obtain a polymer of formula (III) or a polymer of formula (IV):

[0082]

[0083] wherein A, m, n and p are as defined in formula I,

[0084] And R2=-Si(CH3)2CH=CH2,

[0085]

[0086] wherein q is as defined in formula II, and R2=-Si(CH3)2CH=CH2.

[0087] The polymer of formula (III) is an alternating copolymer.

[0088] The polymer of formula (IV) is a homopolymer.

[0089] Thus, the polymer obtained in step c1) may be a poly(dimethyl-co-diethyl)siloxane having the following formula (IIIa):

[0090]

[0091] wherein R2, m, n and p are as defined in formula III, or,

[0092] It may be a poly(methyl hydrogen-co-diethyl)siloxane having the following formula (IIIb):

[0093]

[0094] wherein R2, m, n and p are as defined in formula III.

[0095] The polymers of formula (IIIa) and formula (IIIb) are alternating copolymers.

[0096] Advantageously, the poly(dimethyl-co-diethyl)siloxane of formula (IIIa) has a glass transition temperature (Tg) in the range of -130°C to -142°C, in particular in the range of -135°C to -141°C, more particularly -139°C, the glass transition temperature (Tg) being measured by DSC according to standard ASTM E1356 of May 15, 2014.

[0097] More advantageously, the poly(dimethyl-co-diethyl)siloxane of formula (IIIa) has a weight average molecular weight in the range of 20,000 to 150,000 g / mol, still more advantageously 30,000 to 100,000 g / mol, even more advantageously 40,000 to 80,000 g / mol, in particular 45,000 to 50,000 g / mol, the weight average molecular weight being measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0098] Advantageously, the poly(methylhydrogen-co-diethyl)siloxane of formula (IIIb) has a glass transition temperature ranging from -130°C to -146°C, measured by DSC according to standard ASTM E1356 of 15 May 2014.

[0099] More advantageously, the poly(methylhydrogen-co-diethyl)siloxane of formula (IIIb) has a weight average molecular weight in the range of 300 g / mol to 3500 g / mol, more advantageously 500 g / mol to 3000 g / mol, still more advantageously 1000 g / mol to 2000 g / mol, the weight average molecular weight being measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0100] Advantageously, the poly(ethylmethylsiloxane) of formula (IV) has a glass transition temperature ranging from -130°C to -142°C, measured by DSC according to standard ASTM E1356 of 15 May 2014.

[0101] More advantageously, the poly(ethylmethylsiloxane) of formula (IV) has a weight average molecular weight ranging from 20,000 g / mol to 200,000 g / mol, advantageously from 20,000 g / mol to 150,000 g / mol, as measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0102] The reaction schemes of step c1) (Scheme 5 and Scheme 6) are as follows:

[0103]

[0104] wherein R2, A, m, n and p are as defined above.

[0105]

[0106] wherein R2 and q are as defined above.

[0107] In a specific embodiment, the Lewis acid catalyst is a triflate, advantageously selected from indium (III) triflate, bismuth (III) triflate, aluminum (III) triflate and mixtures thereof, more advantageously indium (III) triflate, and step c1) is carried out in the absence of any solvent, more advantageously at a temperature of 50° C. to 70° C., and still more advantageously the catalyst is present in an amount of 0.1 mg to 2 mg per gram of polymer.

[0108] In another specific embodiment, the Lewis acid catalyst is a perfluoroborane, such as B(C6F5)3, and step c1) is carried out in the absence of any solvent or using toluene as a solvent, more advantageously at room temperature (20°C-25°C), still more advantageously the catalyst is present in an amount of 0.1 mg-1 mg per gram of polymer.

[0109] In another specific embodiment, the Lewis acid catalyst is a mixture of trifluoromethanesulfonate and perfluoroborane, advantageously a mixture of indium(III) trifluoromethanesulfonate and B(C6F5)3, and step c1) is carried out in the absence of any solvent, more advantageously at room temperature (20°C-25°C), and still more advantageously the catalyst is present in an amount of 0.1 mg-1 mg per gram of polymer.

[0110] In another specific embodiment, when step c1) is carried out and perfluoroborane, in particular B(C6F5)3, is further added, the catalyst used in step b) is not removed. Advantageously, step c1) is carried out in the absence of any solvent, more advantageously at room temperature.

[0111] The process according to the invention may comprise a step c2) of adding trialkylsilyl end groups by reacting the polymer obtained in step b) with a trialkylsilane, in particular trimethylsilane or triethylsilane, more particularly triethylsilane, in the presence of a Lewis acid catalyst such as B(C6F5)3 in toluene as solvent, advantageously in order to obtain a polymer of formula (V) or a polymer of formula (VI):

[0112]

[0113] wherein A, m, n and p are as defined in formula I,

[0114] and each R3 independently represents a saturated straight or branched C1-C6 alkyl group, advantageously an ethyl group,

[0115]

[0116] Wherein q is as defined in Formula II,

[0117] And each R3 independently represents a saturated straight or branched C1-C6 alkyl group.

[0118] For the purposes of the present invention, the term "(C1-C6)alkyl" is intended to mean any straight-chain or branched saturated alkyl group having 1 to 6 carbon atoms, in particular the groups CH3 (methyl) and CH2CH3 (ethyl).

[0119] The polymer of formula (V) is a silicone oil and is an alternating copolymer. The polymer of formula (VI) is a silicone oil and is a homopolymer.

[0120] Advantageously, the poly(dimethyl-co-diethyl)siloxane represented by formula (V) has a glass transition temperature (Tg) in the range of -130°C to -145°C, in particular -135°C to -142°C, more particularly -136°C, the glass transition temperature (Tg) being measured by DSC according to standard ASTM E1356 of May 15, 2014.

[0121] More advantageously, the poly(dimethyl-co-diethyl)siloxane represented by formula (V) has a weight average molecular weight in the range of 40,000 g / mol to 65,000 g / mol, still more advantageously 45,000 g / mol to 55,000 g / mol, as measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0122] Advantageously, the poly(ethylmethylsiloxane) of formula (VI) has a glass transition temperature (Tg) ranging from -130°C to -142°C, measured by DSC according to standard ASTM E1356 of 15 May 2014.

[0123] More advantageously, the poly(ethylmethylsiloxane) of formula (VI) has a weight average molecular weight ranging from 20,000 g / mol to 150,000 g / mol, measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018.

[0124] The reaction scheme of step c2) (Scheme 7 and Scheme 8) is as follows:

[0125]

[0126]

[0127] wherein R3, A, m, n and p are as defined above.

[0128]

[0129] wherein R3 and q are as defined above.

[0130] In another specific embodiment, the Lewis acid catalyst is a perfluoroborane, such as B(C6F5)3, and step c2) is carried out without any solvent or using toluene as solvent, more advantageously at room temperature (20°C-25°C), still more advantageously the catalyst is present in an amount of 0.1 mg-1 mg per gram of polymer.

[0131] In another specific embodiment, the process according to the invention comprises, after step c1) or c2), a further step d) of removing the catalyst used in steps b) and c1) or step c2), advantageously by using aluminium oxide.

[0132] Advantageously, the process according to the invention is used to prepare 50 / 50 poly(dimethyl-co-diethyl)siloxane or 50 / 50 poly(methylhydrogen-co-diethyl)siloxane.

[0133] The present invention also relates to a poly(dimethyl-co-diethyl)siloxane of formula (IIIa) as described above, which is advantageously obtainable by the process according to the invention and more advantageously has the following properties:

[0134] The weight average molecular weight ranges from 20,000 g / mol to 150,000 g / mol, more advantageously from 30,000 g / mol to 100,000 g / mol, still more advantageously from 40,000 g / mol to 80,000 g / mol, in particular from 45,000 g / mol to 50,000 g / mol, the weight average molecular weight being measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018, and / or,

[0135] The glass transition temperature ranges from -130°C to -142°C, particularly from -135°C to -141°C, and more particularly -139°C, and the glass transition temperature is measured by DSC according to the standard ASTM E1356 of May 15, 2014.

[0136] The polymer of formula (IIIa) is an alternating copolymer.

[0137] The present invention also relates to a poly(methylhydrogen-co-diethyl)siloxane of formula (IIIb) as described above, which is advantageously obtainable by the process according to the invention and more advantageously has the following properties:

[0138] The weight average molecular weight ranges from 300 g / mol to 3500 g / mol, more advantageously from 500 g / mol to 3000 g / mol, still more advantageously from 1000 g / mol to 2000 g / mol, the weight average molecular weight being measured by the viscosity determination method according to the standard ASTM E3116-18 of January 25, 2018, and / or,

[0139] The range of the glass transition temperature is as follows: -130°C to -146°C, and the glass transition temperature is measured by DSC according to the standard ASTM E1356 of May 15, 2014.

[0140] The polymer of formula (IIIb) is an alternating copolymer.

[0141] The present invention also relates to a poly(dimethyl-co-diethyl)siloxane of formula (V) as described above, which is advantageously obtainable by the process according to the invention, more advantageously having the following properties:

[0142] The weight average molecular weight ranges from 500 g / mol to 150,000 g / mol, advantageously from 1,000 g / mol to 3,000 g / mol, measured by the viscometry method according to standard ASTM E3116-18 of January 25, 2018, and / or,

[0143] The glass transition temperature ranges from -130°C to -145°C, particularly from -135°C to -142°C, and more particularly -139°C, and the glass transition temperature is measured by DSC according to the standard ASTM E1356 of May 15, 2014.

[0144] The polymer of formula (V) is an alternating copolymer.

[0145] The polymer of formula (V) is silicone oil.

[0146] The present invention also relates to a composition for preparing silicone rubber, the composition comprising:

[0147] (A) 60 wt% to 94 wt% of a vinyl-terminated poly(dimethyl-co-diethyl)siloxane represented by formula (IIIa) according to the present invention;

[0148] (B) 5% to 35% by weight of a reinforcing filler, advantageously fumed silica;

[0149] (C) 1% to 5% by weight of a crosslinker having a Tg < -130°C; advantageously having the formula (IIIb) according to the invention;

[0150] (D) a suitable amount of a curing catalyst, advantageously a Pt(0) catalyst such as platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane dissolved in methylvinylcyclosiloxane, and,

[0151] (E) Optional Pt inhibitor, such as 1-ethynyl-1-cyclohexanol.

[0152] In the present application, the term "silicone rubber" should be understood to mean a substance having the ability to maintain elasticity in the temperature range of 200°C to -140°C.

[0153] In the composition according to the present invention, the respective amounts of compound (A) (vinyl-terminated poly(dimethyl-co-diethyl)siloxane of formula (IIIa)) and compound (C) (crosslinker) are controlled by the ratio between the number of units (R'HSiO 2 / 2) and the number of alkenyl groups, and are adjusted accordingly taking into account the relative proportion of the alkenyl moieties in compound (A) and the relative proportion of the units (R'HSiO2 / 2) in compound (C).

[0154] An important feature of the silicone rubber composition according to the invention is the ratio between the number of units (R'HSiO 2 / 2) of compound (C) introduced into the silicone base composition and the number of diethyl groups of compound (A) introduced into the rubber composition. According to the invention, the ratio between the number of units (R'HSiO 2 / 2) and the number of alkenyl groups is greater than 3. Values ​​less than or equal to 3 result in mechanical and adhesive properties of the composition that are insufficient for use as a self-adhesive PDIES silicone on metal surfaces such as stainless steel or titanium.

[0155] Advantageously, this ratio is greater than 4 and less than 25.

[0156] The curing catalyst is a hydrosilylation catalyst, in particular a platinum Pt(0) catalyst, more particularly complexed with a divinyltetraalkylsiloxane ligand, preferably complexed with 1,3-divinyltetramethylsiloxane, such as platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane dissolved in methylvinylcyclosiloxane. Such catalysts are described, for example, in document WO 0142258 A1. Karstedt catalysts are particularly suitable. As in any conventional hydrosilylation reaction, the amount of catalyst in the composition is a catalytic amount. A catalytic amount means, relative to the amount of unsaturation of the olefinic double bond type present in the composition, less than one molar equivalent of platinum. Typically, it is sufficient to introduce less than 1000ppm, and preferably greater than 30ppm of platinum, calculated relative to the total mass of compound (A) and compound (C).

[0157] Compound (C) (R'HSiO 2 / 2 The hydrosilylation reaction of the organopolysiloxane with the alkenyl groups of compound (A) is designed to result in crosslinking of the organopolysiloxane and allow the production of a crosslinked silicone rubber composition. Crosslinking is usually initiated by bringing the silicone rubber composition to a temperature sufficient to allow the hydrosilylation reaction. It is usually carried out at a temperature of 15°C to 200°C, for example 20°C to 150°C, better still 50°C to 150°C.

[0158] In a known manner, crosslinkable silicone compositions generally contain inhibitors. Inhibitors are generally used to control the temperature and time of the hydrosilylation crosslinking reaction, and thereby further control the crosslinking reaction, especially its start and speed. If a crosslinking inhibitor is used, the amount of the inhibitor is preferably 1ppm-50,000ppm relative to the total mass of compound (A) and compound (C), more preferably 20ppm-2000ppm, and particularly 100ppm-1000ppm. As an inhibitor, alkynols such as 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-dodecyn-3-ol, 2-phenyl-3-butyn-2-ol can be used. Preferably, the silicone rubber composition according to the present invention contains an inhibitor.

[0159] The silicone rubber composition according to the invention also has the important feature of comprising a reinforcing filler, which is advantageously a hydrophobic silica, in particular a pyrogenic silica. In a known manner, a hydrophobic silica is a silica whose surface is partially covered by organic groups such as alkyl groups. The silica can be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenic silica. Preferably, the BET specific surface area of ​​the silica is less than 450 m 2 / g, preferably 80m 2 / g-400m 2 / g, especially 100m 2 / g-300m 2 / g, advantageously 150m 2 / g-250m 2 It is also possible to use mixtures of several silicas, for example Aerosil R 8200, Aerosil R 812S, Aerosil E 9200 (from Evonik) or Cab-O-Sil TS 530 (from Cabot).

[0160] In order to make the silicon dioxide hydrophobic, it is known to modify the surface of the silicon dioxide. The modification of the silicon dioxide surface can be obtained in a known manner by reacting the silicon dioxide with a compound carrying a hydrophobic group, such as a trialkylsilyl group, in particular a trimethylsilyl group. Particularly suitable are silicon dioxides whose surface is modified with trimethylsilyl groups. Mention may be made, for example, of those obtained by modification with hexamethyldisilazane.

[0161] The content of hydrophobic silica is adjusted by a person skilled in the art according to its specific surface area and the use of the silicone rubber composition. Preferably, the content of hydrophobic silica in the silicone rubber composition is greater than or equal to 5% of the total weight of silica, compound (A) and compound (C), and less than or equal to 35% of the total weight of silica, compound (A) and compound (C). When the content of hydrophobic silica is lower than 5% of the total weight of silica, compound (A) and compound (C), the reinforcing properties of the composition may not be sufficient for certain applications. When the content of hydrophobic silica exceeds 35% of the total weight of silica, compound (A) and compound (C), silicone rubber formulation may not be possible (solid paste is obtained when using silica HDK H2000 (Wacker) or when using more than 20% by weight of Cab-O-Sil TS 530, Aerosil R 8200 or Aerosil E 9200).

[0162] The silicone rubber composition according to the present invention can be prepared by incorporating hydrophobic silica into compound (A), then adding compound (C) in a mixed state, and finally adding a catalyst. When an inhibitor is used, it is usually added to the mixture of hydrophobic silica and compound (A) before incorporating compound (C).

[0163] The invention also relates to a silicone rubber obtainable by curing the composition according to the invention and as described above and having a glass transition temperature in the range of -130°C to -142°C, advantageously from -135°C to -140°C, in particular -138°C, the glass transition temperature being measured by DSC according to standard ASTM E1356 of 15 May 2014 and / or having no crystallization / melting transition in the range of -140°C to +250°C, measured by DSC according to standard ASTM E1356 of 15 May 2014.

[0164] More advantageously, the silicone rubber according to the invention has an elongation at break higher than 100%, in particular higher than 200%, more particularly higher than 300% and for example 348% (measured by French INSTRON 34TM-10 using standard AFNOR NF T 46002, H2, September 1988).

[0165] Even more advantageously, the silicone rubber according to the invention has a modulus of elasticity of >1 MPa, advantageously >3 MPa, measured with a French INSTRON 34TM-10 according to standard AFNOR NF T 46002 of September 1988.

[0166] Still more advantageously, the silicone rubber according to the invention has a Shore A hardness in the range of 35-40, measured by durometer hardness according to standard ASTM D 2240 of July 23, 2021.

[0167] The present invention also relates to the use of the silicone rubber according to the invention or the poly(dimethyl-co-diethyl)siloxane of formula (V) in the aerospace industry, in particular in space exploration vehicles. More particularly, the present invention also relates to the use of the poly(dimethyl-co-diethyl)siloxane of formula (V) according to the invention as silicone oil for electric motors at low temperatures, in particular below -100°C.

[0168] Finally, the invention relates to the use of the poly(methylhydrogen-co-diethyl)siloxanes according to the invention of the following formula (IIIb) as crosslinkers for the preparation of silicone rubbers.

[0169] The above-mentioned characteristics and others of the present invention will be better understood on reading the following description of several exemplary embodiments of the invention, which are given by way of illustration and not limitation.

[0170] Example 1: Synthesis of poly(diethyl-co-dimethyl)siloxane (50 / 50) (PDIES-50 / 50)

[0171] Step 1 (Step a)

[0172] First, 1 kg of dichlorodiethylsilane (SID3402.0-1KG, Gelest, USA) was distilled into a 2L flask at 40-50°C / 20 mbar vacuum, and the 2L flask was cooled to -79°C using dry ice. The obtained silane was a transparent liquid.

[0173] Without removing oxygen from water in advance, the synthesis of poly (diethyl-to-dimethyl) siloxane (50 / 50) was carried out. An 8L glass cylinder was placed in an ice bath (polypropylene box) and cooled to 0°C-5°C. The reactor was equipped with a bubbler to check the final gas precipitation. Deionized water (3.7L) was added to the glass reactor, which was cooled to 5°C in an ice bath. The stirring was set to 200rpm. Then, 306g of diethyldichlorosilane and 251.37g of dichlorodimethylsilane (ThermoScientific, batch A0439125) were added to a glass column equipped with a Teflon valve (glass was dried under 100°C vacuum and maintained with a slight N2 flow). The silanes were mixed using a Teflon rod and added dropwise to 3.7L water at a rate of about three drops / second. The reaction medium temperature was maintained at 5°C to 7°C. The silane hydrolysis was carried out for two hours at a stirring rate of 300rpm.

[0174] Subsequently, the reactor is placed in a polypropylene water bath heated to 40°C so that the reaction medium temperature is 30°C-35°C, and silanol is further stirred at 300rpm for 2 hours. Then, 1.5L heptane is added to separate silanol from the aqueous phase, and a silicone tube (slight vacuum) is used to pump HCl (aqueous solution) from below the silanol oligomer layer. The silanol oligomer is extracted with 1L heptane, and the reactor and separatory funnel (500ml funnel) are washed with 1.5L heptane in addition. 25g MgSO is added, and the silanol oligomer is dried at 200rpm. Wet MgSO is filtered, and then the silanol oligomer is kept overnight in 2L heptane under nitrogen. At 90°C, a rotary evaporator is used to distill out the organic solvent under vacuum. 313.2g silanol oligomer (theoretical value 369.4g) is obtained, and the productivity is 85%. According to the standard ASTM E3116-18 of January 25, 2018, the viscosity is 35 mPa.s (viscometer model: VSC-N4 (China Bioevopeak) - measuring range: 20 mPa.s-2,000,000 mPa.s).

[0175] The silanol was placed in a 2 L glass flask at 145°C (air, no vacuum) for 120 minutes. The viscosity was measured after 2 hours at 145°C when cooled to 25°C (thermostat). Viscosity: 38 mPa.s. The silanol was purged with nitrogen, closed with a silicone septum in a 1 L container and kept at -20°C (to prevent further condensation with water).

[0176] Step 2 (Step b)

[0177] The silanol oligomer obtained in 298g step 1 is heated at 145 ℃ for 15 minutes, and vacuumized (<2 mbar vacuum) for 30 minutes while hot, until no bubble formation is observed.Then the silanol oligomer is poured into a dry 1L flask equipped with a silicone diaphragm, a magnetic stirrer and a nitrogen stream while hot. Subsequently, under a nitrogen stream, 35mg indium (III) trifluoromethanesulfonate is added to every 100g silanol oligomer. By mixing at 500rpm, the catalyst is dispersed in the silanol oligomer. Then, the reaction is allowed to spend the night (17 hours) in a closed container without stirring. Viscosity increase is observed. The next day, 57mg tris (pentafluorophenyl) borane catalyst (Sigma-Aldrich, #442593) is added under nitrogen, and mixed at 500rpm for 5 minutes, and the reaction is allowed to continue for an additional 24 hours.

[0178] Step 3 (Step c)

[0179] 35 mg of tris(pentafluorophenyl)borane catalyst (Sigma-Aldrich, #442593) was added to the reaction medium, followed by 1.5 ml of vinyldimethylmethoxysilane (AB106075, ABCR, Germany). The reaction medium was mixed for 5 minutes and then continued to react for an additional 5 hours without stirring. Finally, the reaction product was transferred to a rotary evaporator and excess vinyldimethylmethoxysilane and other volatiles were distilled off at 95°C / 30 mbar.

[0180] Step 4: Removal of Catalyst (Step d)

[0181] The siloxane polymer obtained in step 3 is cooled to room temperature, and 150g of neutral alumina (#199974, Sigma Aldrich) is added together with 600ml of heptane. The suspension is stirred at 300rpm for 20 minutes. Solids are then removed by filtering on a 2-porosity ceramic filter, then filtering on a 4-porosity ceramic filter, and finally filtering on a 0.45μm PTFE filter. The solvent is distilled off using a rotary evaporator heated to 95°C and reduced to 30 mbar vacuum. Finally, the siloxane polymer is heated for one hour (vacuum oven) at 150°C and under <1 mbar vacuum. No significant mass loss is measured by DSC at -80°C to 200°C.

[0182] According to the standard ASTM E3116-18 of January 25, 2018, the viscosity is 4012 mPa.s, Mw=45000 g / mol (viscometer model: VSC-N4 (China Bioevopeak), measuring range: 20 mPa.s-2,000,000 mPa.s).

[0183] According to the standard ASTM E1356 of May 15, 2014, Tg=-139°C (2°C / min, N2) was obtained on this material using DSC (model: DSC 3, Mettler Toledo, Switzerland).

[0184] The polydispersity index (PD) was determined by GPC to be 1.63.

[0185] The GPC conditions are as follows:

[0186] GPC (Gel Permeation Chromatography): Agilent 1260 Infinity coupled with 390-MDS detector (Agilent, USA).

[0187] Refractive index detector: 1260 Infinity RID (Agilent, USA).

[0188] The heating device was a Mistral column oven (Spark, The Netherlands).

[0189] The column set consists of:

[0190] 1 pre-set column PSSSDV (PSS / Agilent).

[0191] 2 columns PSSSDV analysis linear XL (PSS / Agilent).

[0192] The polymer samples were dissolved in 1 mL of toluene before injection.

[0193] Toluene, HPLC Plus, for HPLC (#650579-1L, Merck).

[0194] Experimental conditions:

[0195] Eluent: toluene; flow rate: 1 mL / min; temperature: 35°C.

[0196] Calibration was conventional with polystyrene narrow standards ranging from 682 g / mol to 130,000 g / mol.

[0197] The software used for Mw calculation was Cirrus GPC software (Agilent, USA).

[0198] Example 2: Silicone formulation example for preparing silicone rubber:

[0199] 50 g of a siloxane polymer with a Mw of 45500 g / mol (synthesized in steps 1-4 above).

[0200] 15 g of SiO2 (HDK H2000, Wacker, Germany).

[0201] 7 mg of 99% 1-ethynyl-1-cyclohexanol (E51406, Sigma-Aldrich) (Pt inhibitor).

[0202] 140 mg of Pt catalyst* (platinum (0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane complex solution - Sigma Aldrich, #479543).

[0203] 1.35 g of HMS-H271 crosslinker (Gelest, USA) (25%-30% methyl hydrogen-dimethylsiloxane copolymer, hydride terminated, 24 cSt-60 cSt).

[0204] The ingredients were mixed in a mixer at 2000 rpm and cured at 150°C for 1 hour or at room temperature for 24 hours.

[0205] An elastic crosslinked silicone rubber (30% by weight SiO2) is obtained, whose Tg = -138 ° C., which does not show crystallization or melting at -150 ° C to +250 ° C., which is measured by DSC according to the standard ASTM E1356 of May 15, 2014 (model: DSC 3, Mettler Toledo, Switzerland). Shore A hardness: 35-40 (measured using HBA100-0 (Kern, Switzerland, according to ASTM D2240-15 (2021) effective from July 23, 2021)). Elongation at break: 348% (measured by French INSTRON 34TM-10, using the standard AFNOR NF T 46002, H2 of September 1988).

[0206] Example 3: Triethylsilyl-terminated poly(dimethyl-co-diethyl)siloxane (50 / 50) silicone oil

[0207] Step (a): Hydrolysis

[0208] The 1L flask with four inlets, condenser, side arm, exhaust outlet and magnetic bar is filled with 370ml deionized water.Then the device is cooled to 5 ℃, and (with a rate of 3 drops / second) 30.0g dichlorodiethylsilane (Gelest, SID3402.0, Gelest) and 24.6g dichlorodimethylsilane (ThermoScientific, #113312500) (both are cooled to 5 ℃ and mixed) are added dropwise in one hour.The reaction medium is stirred at 600rpm.Subsequently, the reaction temperature is increased to 30 ℃ and stirred for another hour.Add 500ml heptane, then separate silicone from aqueous phase in a separating funnel.Wash the organic phase with deionized water to neutral pH.

[0209] The reaction product in heptane was transferred to a 1 L flask and the residual water was dried using 50 g of anhydrous MgSO4. The product was filtered using a P4 porosity ceramic filter and a 0.45 μm PTFE microfilter. Heptane and volatiles were removed using a rotary evaporator at 90 ° C / reduced to 18 mbar vacuum. At RT, no volatiles were shown under additional vacuum reduced to 1 mbar.

[0210] Step (b): Chain Growth

[0211] Under N2 flow, product is transferred to a dry 100ml round-bottom flask equipped with a magnetic stirring bar. Then 14mg indium trifluoromethanesulfonate (III) is added and stirred for 30 minutes. Then 14mg tris (pentafluorophenyl) borane catalyst (Sigma-Aldrich, #442593) dissolved in 2ml anhydrous toluene (Sigma Aldrich, #244511) is added. Reaction medium is stirred for another 30 minutes.

[0212] Step (c2):

[0213] Finally, 5ml triethylsilane (Sigma 230197-25G) and 6.5mg tris (pentafluorophenyl) borane were dissolved in 1ml toluene. The solution was stirred for 30 minutes until bubbles stopped separating out. Under the constant mixing of 400rpm, the catalyst was adsorbed on 25g neutral Al2O3. The reaction medium was mixed for 10 minutes, then 200ml heptane was added, and the suspension was filtered on P2 and P4 ceramic filters, then filtered on a 0.45μm PTFE microfilter. The solvent was distilled out at 90℃ / 20 millibars, then kept at room temperature <1 millibar vacuum. The composition of the product was confirmed by FTIR and Raman spectroscopy. The glass transition temperature Tg=-140℃ was measured by DSC at a rate of 2℃ / minute under a nitrogen stream.

[0214] Example 4: Triethylsilyl-terminated poly(methylhydrogen-co-diethyl)siloxane (50 / 50) silicone oil (crosslinker)

[0215] Step a): Hydrolysis

[0216] A 1 L flask equipped with four inlets, a condenser, a side arm, a vent outlet and a magnetic stir bar was purged under a slight nitrogen stream at 25° C. Then, under constant stirring at 400 rpm, 22 g of diethyldiethoxysilane (Gelest, SID3404) was added, followed by 16.8 g of methyldiethoxysilane (Sigma-Aldrich, #66612).

[0217] Steps b) and c1)

[0218] Finally, use Pasteur pipette that 7.5mg trifluoromethanesulfonic acid indium (III) catalyst is directly added in the monomer mixture, then at 29 ℃ and 400rpm, draw 11ml deionized water (3 * 3ml+2ml) every 10 minutes.After stirring for one hour, reaction product is transferred in the 250ml flask, and by adding 25g anhydrous MgSO4, moisture is dried.Product is dissolved in 100ml heptane, uses 0.45μm PTFE filter to filter, and uses rotary evaporator to remove volatile matter / solvent under the vacuum of 80 ℃ / reduced to 35 millibars.Under RT, do not show any volatile matter under the additional vacuum of being reduced to 1 millibar.

[0219] Under N2 flow and constant stirring at 400rpm, 7mg tris(pentafluorophenyl)borane catalyst (Sigma-Aldrich, #442593) and 5ml triethylsilane (Sigma 230197-25G) dissolved in 1ml anhydrous toluene (Sigma Aldrich, #244511) were added to the reaction product obtained in the previous step. The solution was stirred for 30 minutes until bubbles stopped separating out. The borane catalyst was adsorbed on 25g neutral Al2O3. The reaction medium was mixed for 10 minutes (magnetic Teflon rod), then 100ml heptane was added, and the suspension was filtered on P2 and P4 ceramic filters, then on a 0.45μm PTFE microfilter. The solvent was distilled off at 90℃ / 20mbar, then kept at room temperature <1mbar vacuum. The composition of the product (clear transparent liquid) was confirmed by FTIR and Raman spectroscopy. The glass transition temperature Tg = -144.7°C was measured by DSC at a rate of 2°C / min under a nitrogen flow.

[0220] Example 5: Synthesis of poly(ethyl-co-methylsiloxane)-PEMS

[0221] Step a (hydrolysis)

[0222] Ethylmethyldichlorosilane (#AB111135, ABCR, Germany) was used as received (97% purity). It appeared as a clear, transparent pink liquid.

[0223] The synthesis was carried out in an air atmosphere. The 20L glass reactor was cooled to 5°C. The 1L side arm for silane addition was equipped with a bubbler and maintained under a slight nitrogen flow during the silane addition. During the addition of chlorosilane, deionized water (1.4L) was cooled and maintained at 4°C-6°C. Stirring was set to 200rpm. First, 213.0g (instead of 210g) of ethylmethyldichlorosilane (3 drops / second) was dripped into 1.4L water. Then, the reaction medium temperature was gradually increased to 30°C and stirred at 200rpm for 2 hours and 30 minutes. A transparent silanol layer was formed on the water surface.

[0224] The silanol was extracted with 1.25 L of heptane and dried with 250 g of MgSO4. Heptane was distilled off using a rotary evaporator at 90-95 ° C and then kept at 1 mbar vacuum at room temperature. The viscosity of the silanol obtained was 31.7 mPa.s. The silanol in the 1 L round-bottomed flask was then placed in an oven at 145 ° C for 20 minutes. The silanol was cooled to RT. Subsequently, 100 mg of indium (III) trifluoromethanesulfonate was added under constant stirring at 200 rpm. The silanol was then allowed to polymerize over the weekend. 115.0 g of silicone (theoretical value 131.83 g) was obtained with a productivity of 87%.

[0225] Step b (chain growth)

[0226] 50 g of the PEMS silanol obtained in step a) was mixed with 50 mg of indium (III) trifluoromethanesulfonate (#422151, Sigma-Aldrich), stirred at 200 rpm for 5 minutes, and allowed to polymerize (without stirring) during the weekend. Subsequently, water and volatiles were removed from the silicone using a rotary evaporator at 95 ° C under a vacuum of 30 mbar. The silanol was then mixed with 125 g of anhydrous MgSO4 and dissolved in 400 ml of heptane. The solid was filtered on a P4 ceramic filter and heptane was distilled off at 95 ° C. The silanol was heated at 145 ° C for 10 minutes under a vacuum of 1 mbar. The silanol was then cooled to room temperature, and 25 mg of tris (pentafluorophenyl) borane was added, followed by 2 ml of toluene, mixed for 2 minutes, and kept in a 1 L flask closed with a silicone septum under an N2 atmosphere (without stirring). The silanol was allowed to polymerize overnight.

[0227] Step c1

[0228] The silanol obtained in step b is heated to 95°C under 25 mbar vacuum to remove water and volatiles. Subsequently, 0.33g of 98% vinyl-1,1,3,3-tetramethyldisiloxane (SIV9097.5, Gelest, USA) and 25mg of 95% tris(pentafluorophenyl)borane (#442593, Sigma Aldrich) are added, followed by 2ml of toluene. Silicone is mixed at 200rpm for 5 minutes and reacted at 25°C for 2 hours. Finally, a vacuum line is connected and volatiles are distilled out at 95°C under 30 mbar vacuum. Silicone is diluted in 200ml hexane and mixed with 25g Al2O3 (neutral alumina), and the suspension is mixed for 10 minutes. The catalyst adsorbed on alumina is removed by filtering on a P4 ceramic filter and then filtering on a 0.45μm PTFE microfilter. The solvent was distilled off using a rotary evaporator at 95° C. and the polymer was transferred to a dry 250 ml glass flask and subjected to a vacuum of 1 mbar at 150° C. and then at 170° C. (20 minutes each). The viscosity was 5500 mPa.s.

[0229] The obtained material was subjected to DSC analysis, measured at 2°C / min under N2, Tg = -141°C. FTIR and Raman measurements showed the absence of cyclic products. The FTIR and Raman spectra of the product were consistent with the PEMS spectra calculated at the B3LYP / 6-311G (d, p) level (Gaussian16).

[0230] According to the standard ASTM E3116-18 of January 25, 2018, the viscosity is 25 mPa.s, Mw = 2000 g / mol (viscometer model: VSC-N4 (China Bioevopeak), measuring range: 20 mPa.s-2,000,000 mPa.s).

[0231] The polydispersity index (PD) was determined by GPC to be 2.41. The GPC conditions were the same as in Example 1.

[0232] Crosslinking: 5 g PEMS silicone (step c1), 1.5 g SiO2 (HDK H2000), 14 mg Pt(0) in tetravinylcyclotetrasiloxane (#479543, Sigma Aldrich), 135 mg HMS H271 (Gelest, USA) at 35°C overnight, then at 150°C for 20 minutes.

[0233] An elastic crosslinked silicone rubber is obtained which has a Tg = -139°C and exhibits no crystallization or melting behavior between -139°C and +250°C.

[0234] No silicone crystallization was observed from +25°C to -130°C at 2°C / min under N2.

Claims

1. A method for preparing a polysiloxane containing a methyl group and an ethyl group, the method comprising the following steps: a) hydrolysis reaction of silanol precursor; b) chain extension of the silanol-terminated siloxane oligomer obtained in step a) by Lewis acid-induced polycondensation by addition of a triflate catalyst, in particular indium(III) triflate, followed by addition of a perfluoroborane catalyst, in particular tris(pentafluorophenyl)borane.

2. The method according to claim 1, characterized in that The polysiloxane containing methyl and ethyl groups is selected from the group consisting of: Poly(dimethyl-co-diethyl)siloxane or poly(methyl hydrogen-co-diethyl)siloxane represented by the following formula (I): Where A represents a methyl group or a hydrogen atom, m and n represent the molar percentages of the repeating units –O-Si(Me)(A) and –O-Si(Et2), respectively. m = 0.5-0.8, n = 0.2-0.5, and m + n = 1, p represents the number of the two repeating units so as to obtain a weight average molecular weight in the range of 20000 g / mol to 150000 g / mol when A represents a methyl group and in the range of 300 g / mol to 3500 g / mol when A represents a hydrogen atom, and Poly(ethylmethylsiloxane) represented by the following formula (II): Where q represents the number of repeating units.

3. The method according to claim 2, characterized in that The silanol precursor of step a) is selected from (R1)2ethylmethylsilane, a mixture of (R1)2dimethylsilane and (R1)2diethylsilane, and a mixture of (R1)2methylsilane and (R1)2diethylsilane, wherein R1 represents a chlorine atom, a (C1-C6)alkoxy group, an acetoxy group or an oxime group, and advantageously R1 represents a chlorine atom, a methoxy group or an ethoxy group.

4. The method according to any one of claims 1 to 3, characterized in that The indium(III) trifluoromethanesulfonate catalyst is present in an amount of 0.1 mg to 1 mg per gram of oligomer.

5. The method according to any one of claims 1 to 4, characterized in that Step b) is carried out at room temperature.

6. The method according to any one of claims 1 to 5, characterized in that Step b) is carried out in bulk, without any solvent.

7. The method according to any one of claims 2 to 6, characterized in that: The poly(dimethyl-co-diethyl)siloxane obtained in step b) has a weight average molecular weight ranging from 20000 g / mol to 150000 g / mol, The poly(methylhydrogen-co-diethyl)siloxane obtained in step b) has a weight average molecular weight ranging from 300 g / mol to 3500 g / mol, and, The poly(ethylmethylsiloxane) obtained in step b) has a weight average molecular weight ranging from 1000 g / mol to 200000 g / mol.

8. The method according to any one of claims 1 to 7, characterized in that The process also comprises a step c1) of adding vinyl end groups by reacting the polymer obtained in step b) with vinyldimethylmethoxysilane or vinyl-1,1,3,3-tetramethyldisiloxane in the presence of a Lewis acid catalyst, such as indium(III) triflate without any solvent, or B(C6F5)3 in toluene as solvent or without any solvent, or a mixture of indium(III) triflate and B(C6F5)3, at a temperature ranging from 20°C to 70°C, advantageously in order to obtain: A polymer having the following formula (III): wherein A, m, n and p are as defined in formula I, And R2=-Si(CH3)2CH=CH2, Alternatively, a polymer having the following formula (IV): wherein q is as defined in formula II, and R2=-Si(CH3)2CH=CH2.

9. The method according to claim 8, characterized in that: The poly(dimethyl-co-diethyl)siloxane obtained in step c1) has a glass transition temperature in the range of -130°C to -142°C, The poly(methylhydrogen-co-diethyl)siloxane obtained in step c1) has a glass transition temperature in the range of -130°C to -146°C, and The poly(ethylmethylsiloxane) obtained in step c1) has a glass transition temperature in the range of -130°C to -142°C.

10. The method according to any one of claims 1 to 7, characterized in that The process also comprises a step c2) of adding trialkylsilyl end groups by reacting the polymer obtained in step b) with a trialkylsilane in the presence of a Lewis acid catalyst, such as B(C6F5)3 in toluene as solvent, advantageously in order to obtain: A polymer having the following formula (V): wherein A, m, n and p are as defined in formula I, and each R3 independently represents a saturated straight or branched C1-C6 alkyl group, Alternatively, a polymer having the following formula (VI): Wherein q is as defined in Formula II, And each R3 independently represents a saturated straight or branched C1-C6 alkyl group.

11. The method according to any one of claims 2 to 10, characterized in that The method is used to prepare 50 / 50 poly(dimethyl-co-diethyl)siloxane or 50 / 50 poly(methylhydrogen-co-diethyl)siloxane.

12. A poly(dimethyl-co-diethyl)siloxane having: The following formula (IIIa): wherein R2, m, n and p are as defined in formula III, a weight average molecular weight ranging from 20,000 g / mol to 150,000 g / mol, and A glass transition temperature in the range of -130°C to -142°C can advantageously be obtained by the method according to any one of claims 8, 9 and 11.

13. A poly(methyl hydrogen-co-diethyl)siloxane having: The following formula (IIIb): wherein R2, m, n and p are as defined in formula III, A weight average molecular weight ranging from 300 g / mol to 3500 g / mol, and A glass transition temperature in the range of -130°C to -146°C can advantageously be obtained by the method according to any one of claims 8, 9 and 11.

14. A poly(dimethyl-co-diethyl)siloxane having: The following formula (V): wherein R3, A, m, n and p are as defined in claim 10, A weight average molecular weight ranging from 500 g / mol to 150,000 g / mol, and A glass transition temperature in the range of -130°C to -145°C can advantageously be obtained by the method according to any one of claims 10 and 11.

15. A composition for preparing silicone rubber, the composition comprising: (A) 60 wt% to 94 wt% of a vinyl-terminated poly(dimethyl-co-diethyl)siloxane of formula (IIIa) according to claim 12; (B) 5% to 35% by weight of a reinforcing filler, advantageously fumed silica; (C) 1% to 5% by weight of a crosslinker having a Tg < -130°C; advantageously having the formula (IIIb) according to claim 13; (D) a suitable amount of a curing catalyst, advantageously a Pt(0) catalyst such as platinum(0)-2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane dissolved in methylvinylcyclosiloxane, and, (E) Optional inhibitor, such as 1-ethynyl-1-cyclohexanol.

16. A silicone rubber obtainable by curing the composition according to claim 15 and having a glass transition temperature in the range of -130°C to -142°C, no crystallization / melting transition in the range of -140°C to +250°C and an elongation at break higher than 100%.

17. Use of the silicone rubber according to claim 15 or the poly(dimethyl-co-diethyl)siloxane of formula (V) according to claim 14 in the aerospace industry, in particular in space exploration vehicles.

18. Use of the poly(methylhydrogen-co-diethyl)siloxane of formula (IIIb) according to claim 13 as a crosslinking agent for the preparation of silicone rubber.

Citation Information

Cited By

  • Polyorganosiloxane with regular structure and preparation method thereof

    CN119751875A