Aldehyde modified silicone oil, preparation method and application
Through hydrosilation reaction and amine-aldehyde condensation reaction, aldehyde-modified silicone oil is prepared for the preparation of hydrophobic coatings, which solves the application limitations of existing silicone oils and achieves efficient and simple preparation of hydrophobic coatings with good curing performance and hydrophobic properties.
Patent Information
- Application Number
- CN202410829032.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-25
Smart Images

Figure CN118772412A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of organosilicon-modified silicone oil, and specifically relates to an aldehyde-modified silicone oil, a preparation method and application thereof. Background Art
[0002] Modified silicone oil refers to a product in which the methyl groups on the silicone oil molecular chain are replaced with organic groups or functional polymer segments, thereby changing the original properties of the silicone oil. Modified silicone oil inherits the advantages of ordinary silicone oil such as aging resistance, demolding, high and low temperature resistance and physiological inertness, and also has a series of properties that ordinary silicone oil does not have, such as easy emulsification, adsorption, biocompatibility and wettability. The performance and application of modified silicone oil vary depending on the functional groups introduced. Common modified silicone oils include amino-modified silicone oil, polyether-modified silicone oil, epoxy-modified silicone oil, phenyl silicone oil, vinyl silicone oil, etc. The invention patent with publication number CN117327282A discloses a method for preparing amino-modified silicone oil, which comprises: (1) mixing an amine compound, acetic acid and propionic acid, and reacting them at a certain temperature for a certain time to obtain a modified ammonium salt; (2) mixing 1,1,3,3-tetramethyl-1,3-di[3-(oxiranylmethoxy)propyl]disiloxane with the modified ammonium salt, and reacting them at a certain temperature for a certain time to obtain an aminosiloxane intermediate; (3) mixing octamethylcyclotetrasiloxane, a catalyst and the aminosiloxane intermediate, and reacting them at a certain temperature for a certain time to obtain an amino-modified silicone oil. The target product prepared by the preparation method has a controllable structure, no solvent is involved in the reaction, has good wettability and stability, and has high reaction production efficiency. The invention patent with publication number CN115368574A discloses a modified silicone oil, a preparation method and its application, wherein alkyl-terminated allyl polyether, unterminated allyl polyether and aromatic allyl ether are used to modify hydrogen-containing polysiloxane to obtain a modified silicone oil shown in Formula 1. The surface, internal pore structure and dimensional stability of a one-component polyurethane foam can be effectively regulated, providing a new idea for the synthesis of an organosilicon surfactant for a one-component polyurethane foam sealant; at the same time, the preparation method of the surfactant is simple, easy to operate and suitable for industrial production. However, the above-mentioned amino- and ether-modified silicone oils have certain limitations in application.
[0003] Aldehyde is a chemical group with active structure and strong reactivity. It has wide applications in many fields such as organic synthesis, biochemistry and materials science. Among them, amine-aldehyde condensation reaction is an important chemical reaction, which mainly involves the reaction between carbonyl-containing aldehydes or ketones and amino-containing compounds (such as amines). The conditions required for this type of reaction are simple and can be carried out at room temperature. Introducing aldehyde groups into silicone oil will bring new properties and functions to silicone oil. Therefore, it is necessary to develop an aldehyde-modified silicone oil. Summary of the invention
[0004] The present invention provides an aldehyde-modified silicone oil, a preparation method and an application thereof. Aldehyde groups are selectively introduced into silicone oil through a hydrosilylation reaction to obtain the aldehyde-modified silicone oil. The aldehyde-modified silicone oil is cross-linked and cured with a diamine compound through an amine-aldehyde reaction, and can be used to prepare a hydrophobic coating.
[0005] The technical solution of the present invention is:
[0006] In a first aspect, a method for preparing an aldehyde-modified silicone oil is disclosed, comprising the following steps:
[0007] 1) Add olefinic aldehyde and terminal hydrogen-containing silicone oil into a reactor, heat it to 50-70°C, add a catalyst, introduce N2, heat it to 70-120°C, stir and react for 3-10h to obtain a crude aldehyde silicone oil;
[0008] 2) The crude product obtained in step 1) is quenched with 1-ethynylcyclohexanol to remove the catalyst, and low-boiling substances are removed by reduced pressure distillation to obtain aldehyde-modified silicone oil.
[0009] Preferably, the alkenal is selected from one of 10-undecenal, 8-undecenal, 9-undecenal, 2-undecenal, decenal, octenal, acrolein, 4-pentenal, 2-pentenal, 7-octenal, 9-decenal, 3-pentenal, isopentenal, isobutyleneal, 2-butenal, 2-hexenal, 2-decenal, 8-nonenal, 2-dodecenal, 8-undecenal, 2-propylacrolein, 4-hexenal, 2-benzylacrolein, 2-ethylacrolein, 2-heptenal, 2-decenal, 7-decenal, 4-decenal, 2-nonenal, 6-nonenal, and 5-octenal.
[0010] Preferably, the terminal hydrogen-containing silicone oil is a low-end hydrogen-containing silicone oil, and the hydrogen content in the terminal hydrogen-containing silicone oil is selected from one of 0.01-0.015%, 0.04-0.05%, 0.06-0.08%, 0.1-0.12%, 0.11-0.13%, and 0.17-0.19%.
[0011] Preferably, in step 1), the molar ratio of olefinic aldehyde to terminal hydrogen-containing silicone oil is (1.05-1.3):1.
[0012] Preferably, the amount of catalyst used in step 1) is 5ppm-20ppm of the total mass of olefinic aldehyde and terminal hydrogen-containing silicone oil.
[0013] Preferably, the amount of 1-ethynylcyclohexanol used in step 2) is 1 / 30-1 / 20 of the mass of the catalyst, more preferably 1 / 25.
[0014] Preferably, the catalyst in step 1) is PT-5000YB catalyst produced by Guangzhou Siyou New Material Technology Co., Ltd.
[0015] In a second aspect, the aldehyde-modified silicone oil prepared by the preparation method of the aldehyde-modified silicone oil is disclosed.
[0016] In a third aspect, the use of the aldehyde-modified silicone oil in preparing a hydrophobic coating is disclosed. The method for preparing the hydrophobic coating comprises the following steps:
[0017] S1 is respectively prepared with ethyl acetate solution of aldehyde-modified silicone oil and diethylenetriamine;
[0018] S2: spraying the ethyl acetate solution of aldehyde-modified silicone oil and the ethyl acetate solution of diethylenetriamine on the surface of the glass sheet in sequence, placing it at 25-30° C. until the surface liquid solidifies, thereby obtaining the hydrophobic coating material.
[0019] Preferably, in step S1, the mass concentration of the aldehyde-modified silicone oil is 50-55%, and the mass concentration of diethylenetriamine is 50-55%.
[0020] First, different aldehyde chain segments are introduced into the end groups of hydrogen-containing silicone oil through the hydrosilylation reaction, and cross-linked copolymerization with diamine compounds is carried out through the amine-aldehyde condensation reaction. After curing, a transparent hydrophobic coating material with hydrophobic properties is obtained. As a low-surface-energy organic silicon material, the introduction of this coating reduces the surface free energy of the glass and increases the roughness of the glass surface, thus playing a hydrophobic role.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The silicone oil prepared by the present invention has good reactivity and can react with a diamine compound to form a film at room temperature to obtain a hydrophobic coating. The hydrophobic coating has good curing performance, is non-sticky after curing, and has a suitable curing time of 20-23h. The contact angle between the glass with the hydrophobic coating of the present invention and water can reach 114.8°, showing good hydrophobic performance.
[0023] 2. The aldehyde-modified silicone oil prepared by the present invention has a simple process and does not have technical problems such as complicated process and high cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the infrared structure of the aldehyde-modified silicone oil prepared in Example 1 of the present invention.
[0025] Figure 2 Schematic diagram of the contact angle between the hydrophobic coating prepared in Example 1 of the present invention and glass.
[0026] Figure 3 It is a schematic diagram of the infrared structure of the aldehyde-modified silicone oil prepared in Comparative Example 1 of the present invention.
[0027] Figure 4It is a schematic diagram of the infrared structure of the aldehyde-modified silicone oil prepared in Comparative Example 2 of the present invention.
[0028] Figure 5 It is a schematic diagram of the contact angle between the uncoated glass and water in Comparative Example 5 of the present invention. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0030] The preparation method of 50% ethyl acetate solution of aldehyde-modified silicone oil and diethylenetriamine is as follows: weigh 20g of aldehyde-modified silicone oil and 20g of diethylenetriamine respectively and put them into a 100ml spray bottle, add 20g of ethyl acetate respectively, mix well and set aside.
[0031] Example 1
[0032] Weigh 4.64g (27.6mmol) 10-undecenal and 40g (24mmol) terminal hydrogenated silicone oil (hydrogen content 0.06-0.08%, purchased from Ningbo Runhe High-tech Materials Technology Co., Ltd.) into the reactor, heat to 70°C, add 0.0893g (10ppm in terms of platinum) Karsted catalyst (PT-5000YB catalyst produced by Guangzhou Siyou New Materials Technology Co., Ltd.), introduce N2, heat to 90°C and stir for 5h to obtain crude aldehyde silicone oil, add 0.0036g 1-ethynylcyclohexanol to quench the catalyst, remove low-boiling substances by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa, and wait until the mass no longer changes to obtain undecenal modified silicone oil. The viscosity (25°C) is 74mPa·S. Figure 1 As shown in the figure, (a) is the infrared spectrum of the mid-range hydrogenated silicone oil in this embodiment, (b) is the infrared spectrum of the undecylenic aldehyde modified silicone oil prepared in this embodiment, 914cm -1 and 2123cm -1 Deformation and stretching vibrations of Si-H, 1726 cm -1 Attributed to -CHO, 1650cm -1 There is no absorption peak attributed to -C=C nearby. From the infrared spectra before and after the reaction, it can be seen that Si-H disappears after the reaction, indicating that the reaction is complete, and -CHO appears, indicating that the reaction occurs and Si-H selectively adds to -C=C.
[0033] Preparation of hydrophobic coating:
[0034] Undecene aldehyde modified silicone oil and 50% ethyl acetate solutions of diethylenetriamine were prepared respectively to form silicone oil solution and diethylenetriamine solution, and were placed in spray bottles respectively. The silicone oil solution was first evenly sprayed on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded. The specific contact angle between the glass with the hydrophobic coating and water is shown in Table 1. Figure 2 shown.
[0035] Example 2
[0036] Weigh 2.92g (52mmol) of acrolein and 40g (40mmol) of terminal hydrogenated silicone oil (hydrogen content 0.1-0.12%) into a reactor, heat to 50°C, add 0.0858g (10ppm) of Karsted catalyst, introduce N2, heat to 70°C and stir for 4h to obtain crude aldehyde silicone oil, add 0.0042g of 1-ethynylcyclohexanol to quench the catalyst, remove low-boiling substances by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa, and wait until the mass no longer changes to obtain acrolein modified silicone oil. The viscosity (25°C) is 50mPa·S.
[0037] Preparation of hydrophobic coating:
[0038] A 50% ethyl acetate solution of acrolein-modified silicone oil and diethylenetriamine were prepared respectively to form a silicone oil solution and a diethylenetriamine solution, which were placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The curing time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0039] Example 3
[0040] 2.96g (19.2mmol) 9-decenal and 40g (16mmol) terminal hydrogenated silicone oil (hydrogen content 0.04-0.06%) were weighed and added to the reactor, the temperature was raised to 60°C, 0.1289g (15ppm) Karsted catalyst was added, N2 was introduced, the temperature was raised to 100°C and stirred for 10h to obtain crude aldehyde silicone oil, 0.0043g 1-ethynylcyclohexanol was added to quench the catalyst, low boiling points were removed by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa, and the mass was no longer changed to obtain 9-decenal modified silicone oil. The viscosity (25°C) was 61mPa·S.
[0041] Preparation of hydrophobic coating:
[0042] 9-decenal modified silicone oil and 50% ethyl acetate solutions of diethylenetriamine were prepared respectively to form silicone oil solutions and diethylenetriamine solutions, which were placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass sheet was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0043] Example 4
[0044] 0.84g (5mmol) 2-undecene aldehyde and 40g (4mmol) terminal hydrogenated silicone oil (hydrogen content 0.01-0.015%) were weighed and added to the reactor, the temperature was raised to 60°C, 0.1634g (20ppm) Karsted catalyst was added, N2 was introduced, the temperature was raised to 120°C and stirred for 9h to obtain crude aldehyde silicone oil, 0.0065g 1-ethynyl cyclohexanol was added to quench the catalyst, low boiling points were removed by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa, and the mass was no longer changed to obtain 2-undecene aldehyde modified silicone oil. The viscosity (25°C) was 78mPa·S.
[0045] Preparation of hydrophobic coating:
[0046] 2-Undecenal-modified silicone oil and 50% ethyl acetate solutions of diethylenetriamine were prepared respectively to form silicone oil solutions and diethylenetriamine solutions, which were placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0047] Example 5
[0048] 7.08g (48.4mmol) of 2-benzyl acrolein and 40g (44mmol) of terminal hydrogenated silicone oil (hydrogen content 0.11-0.13%) were weighed and added to the reactor, the temperature was raised to 50°C, 0.0942g (10ppm) of Karsted catalyst was added, N2 was introduced, the temperature was raised to 110°C and stirred for 7h to obtain crude aldehyde silicone oil, 0.0037g of -ethynyl cyclohexanol was added to quench the catalyst, and low-boiling substances were removed by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa until the mass no longer changed to obtain 2-benzyl acrolein modified silicone oil. The viscosity (25°C) was 89mPa·S.
[0049] Preparation of hydrophobic coating:
[0050] 2-Benzyl acrolein modified silicone oil and 50% ethyl acetate solutions of diethylenetriamine were prepared respectively to form silicone oil solutions and diethylenetriamine solutions, which were placed in spray bottles respectively. The silicone oil solution was first evenly sprayed on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0051] Example 6
[0052] Weigh 6.01g (71.4mmol) of 2-ethylacrolein and 40g (68mmol) of terminal hydrogenated silicone oil (0.17-0.19%) into a reactor, heat to 70°C, add 0.1380g (15ppm) of Karsted catalyst, introduce N2, heat to 80°C and stir for 8h to obtain crude aldehyde silicone oil, add 0.0046g of 1-ethynylcyclohexanol to quench the catalyst, remove low-boiling substances by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa, and wait until the mass no longer changes to obtain 2-ethylacrolein modified silicone oil. The viscosity (25°C) is 68mPa·S.
[0053] Preparation of hydrophobic coating:
[0054] 2-Benzyl acrolein modified silicone oil and 50% ethyl acetate solutions of diethylenetriamine were prepared respectively to form silicone oil solutions and diethylenetriamine solutions, which were placed in spray bottles respectively. The silicone oil solution was first evenly sprayed on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0055] Example 7
[0056] 1.85g (26.4mmol) of methacrolein and 40g (24mmol) of terminal hydrogenated silicone oil (0.06-0.08%) were weighed and added to a reactor, the temperature was raised to 60°C, 0.0419g (5ppm) of Karsted catalyst was added, N2 was introduced, the temperature was raised to 90°C and stirred for 6h to obtain a crude aldehyde silicone oil, 0.0021g of 1-ethynylcyclohexanol was added to quench the catalyst, and low-boiling substances were removed by reduced pressure distillation at 150°C at a vacuum degree of less than -0.95MPa until the mass no longer changed to obtain methacrolein modified silicone oil. The viscosity (25°C) was 76mPa·S.
[0057] Preparation of hydrophobic coating:
[0058] Isopropylamine-modified silicone oil and 50% ethyl acetate solutions of diethylenetriamine were prepared respectively to form silicone oil solutions and diethylenetriamine solutions, which were placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The curing time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0059] Comparative Example 1
[0060] 4.04 g (24 mmol) of 10-undecenal and 40 g (24 mmol) of terminal hydrogenated silicone oil (hydrogen content 0.06-0.08%) were weighed and added to a reactor, the temperature was raised to 70° C., 0.0881 g (10 ppm, it should be noted that 10 ppm is one hundred thousandth of the mass of the added raw material) of Karsted catalyst was added, N2 was introduced, the temperature was raised to 90° C. and stirred for reaction for 5 h, 0.0036 g of 1-ethynylcyclohexanol was added to quench the catalyst, and low boiling points were removed by reduced pressure distillation at 150° C. under a vacuum degree of less than -0.95 MPa. When the mass no longer changed, a modified silicone oil was obtained, such as Figure 3 As shown, 914cm -1 and 2123cm -1 The absorption peaks attributed to the deformation and stretching vibration of Si-H did not completely disappear, indicating that Si-H was not completely reacted.
[0061] Preparation of hydrophobic coating:
[0062] 50% ethyl acetate solutions of modified silicone oil and diethylenetriamine were prepared respectively to form silicone oil solution and diethylenetriamine solution, and placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The curing time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0063] Comparative Example 2
[0064] 5.65 g (33.98 mmol) of 10-undecenal and 40 g (24 mmol) of terminal hydrogenated silicone oil (hydrogen content 0.06-0.08%) were weighed and added to a reactor, the temperature was raised to 70°C, 0.0913 g (10 ppm) of Karsted catalyst was added, N2 was introduced, the temperature was raised to 90°C and stirred for reaction for 5 h, 0.0037 g of 1-ethynylcyclohexanol was added to quench the catalyst, and low boiling substances were removed by reduced pressure distillation at 150°C under a vacuum degree of less than -0.95 MPa. When the mass no longer changed, a modified silicone oil was obtained, such as Figure 4 As shown, 914cm-1 and 2123cm -1 The absorption peak attributed to Si-H disappears, 1645cm -1 An absorption peak attributed to -C=C appears at , indicating that the Si-H reaction is complete but C=C is not completely consumed.
[0065] Preparation of hydrophobic coating:
[0066] 50% ethyl acetate solutions of modified silicone oil and diethylenetriamine were prepared respectively to form silicone oil solution and diethylenetriamine solution, and placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The curing time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0067] Comparative Example 3
[0068] The undecenal-modified silicone oil in Example 1 was replaced with 10-undecenal.
[0069] Preparation of hydrophobic coating:
[0070] 50% ethyl acetate solutions of 10-undecenal and diethylenetriamine were prepared respectively to form silicone oil solution and diethylenetriamine solution, and placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0071] Comparative Example 4
[0072] The undecenal-modified silicone oil in Example 1 is replaced with the terminal hydrogen-containing silicone oil in Example 1 having a hydrogen content of 0.06-0.08%.
[0073] Preparation of hydrophobic coating:
[0074] 50% ethyl acetate solutions of end-hydrogenated silicone oil and diethylenetriamine were prepared respectively to form silicone oil solution and diethylenetriamine solution, and placed in spray bottles respectively. The silicone oil solution was first sprayed evenly on a 50 mm × 50 mm glass, and then the diethylenetriamine solution was sprayed. The glass piece was placed at 25°C until the surface liquid was completely solidified, and a colorless transparent film was formed on the glass surface. The solidification time and the contact angle between water and the glass surface were recorded, as shown in Table 1.
[0075] Comparative Example 5
[0076] In this comparative example, the glass was not treated, and the contact angle between water and the glass surface was as shown in Table 1 and Figure 5 shown.
[0077] Comparative Example 6
[0078] 4.64 g (27.6 mmol) of 10-undecenal and 40 g (24 mmol) of terminal hydrogen (hydrogen content 0.06-0.08%) were weighed and added to the reactor, and 0.0893 g (10 ppm based on platinum) of Karsted catalyst was added, N2 was introduced, and the temperature was raised to 90°C and stirred for 5 hours. In this comparative example, the catalyst was directly added at room temperature without preheating the temperature, and the reaction did not occur when the temperature was raised again.
[0079] Comparative Example 7
[0080] The difference from Example 1 is that diethylenetriamine is replaced by ethylenediamine in this comparative example, and the other preparation methods and steps are the same as those in Example 1.
[0081] Table 1
[0082] Curing time / h Contact angle Example 1 21 114.8° Example 2 20 95.5° Example 3 22 101.2° Example 4 21.5 102.5° Example 5 23 106.5° Example 6 21 89.5° Example 7 21.5 92.5° Comparative Example 1 30, sticky after curing 103.6° Comparative Example 2 35, sticky after curing 85.2° Comparative Example 3 Not solidified -- Comparative Example 4 Not solidified -- Comparative Example 5 -- 77.2° Comparative Example 6 -- -- Comparative Example 7 19 98.5°
[0083] The aldehyde-modified silicone oil prepared by the embodiment of the present invention 1-7 has good reactivity, can react with diethylenetriamine at room temperature to form a film, and obtain a hydrophobic coating, which has good curing properties, is not sticky after curing, and has a suitable curing time of 20-23h, and the contact angle between the glass and water without treatment in the comparative example 5 is 77.2 °, and the contact angle range between the glass and water with the embodiment of the present invention 1-7 hydrophobic coating 1-7 is between 92.5 ° and 114.8 °, showing good hydrophobic properties. The feed ratio of the end-hydrogenated silicone oil and 10-undecene aldehyde is changed respectively in the comparative example 1-2, and the aldehyde-modified silicone oil obtained is not completely reacted, and the prepared hydrophobic coating has a long curing time, and there is a sticky phenomenon, and the contact angle is small. In the comparative example 3-4, the undecene aldehyde modified silicone oil is replaced with 10-undecene aldehyde and the end-hydrogenated silicone oil, and the prepared hydrophobic coating is not cured. In the comparative example 7, diethylenetriamine is replaced with ethylenediamine, and although the curing time is shortened, the hydrophobic property decreases.
[0084] Although the present invention has been described in detail by combining the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing aldehyde-modified silicone oil, characterized in that: The following steps are involved: 1) Add olefinic aldehyde and terminal hydrogen-containing silicone oil into a reactor, heat it to 50-70°C, add a catalyst, introduce N2, heat it to 70-120°C, stir and react for 3-10h to obtain a crude aldehyde silicone oil; 2) The crude product obtained in step 1) is quenched with 1-ethynylcyclohexanol to remove the catalyst, and low-boiling substances are removed by reduced pressure distillation to obtain aldehyde-modified silicone oil.
2. The method for preparing the aldehyde-modified silicone oil according to claim 1, characterized in that: The alkenal is selected from one of 10-undecenal, 8-undecenal, 9-undecenal, 2-undecenal, decenal, octenal, acrolein, 4-pentenal, 2-pentenal, 7-octenal, 9-decenal, 3-pentenal, isopentenal, isobutyleneal, 2-butenal, 2-hexenal, 2-decenal, 8-nonenal, 2-dodecenal, 8-undecenal, 2-propylacrolein, 4-hexenal, 2-benzylacrolein, 2-ethylacrolein, 2-heptenal, 2-decenal, 7-decenal, 4-decenal, 2-nonenal, 6-nonenal, and 5-octenal.
3. The method for preparing the aldehyde-modified silicone oil according to claim 1, characterized in that: The terminal hydrogen-containing silicone oil is a low-end hydrogen-containing silicone oil, and the hydrogen content in the terminal hydrogen-containing silicone oil is selected from one of 0.01-0.015%, 0.04-0.05%, 0.06-0.08%, 0.1-0.12%, 0.11-0.13%, and 0.17-0.19%.
4. The method for preparing the aldehyde-modified silicone oil according to claim 1, characterized in that: In step 1), the molar ratio of olefinic aldehyde to terminal hydrogen-containing silicone oil is (1.05-1.3):
1.
5. The method for preparing the aldehyde-modified silicone oil according to claim 1, characterized in that: The amount of catalyst used in step 1) is 5ppm-20ppm of the total mass of olefinic aldehyde and terminal hydrogen-containing silicone oil.
6. The method for preparing the aldehyde-modified silicone oil according to claim 1, characterized in that: In step 2), the amount of 1-ethynylcyclohexanol used is 1 / 30-1 / 20 of the mass of the catalyst.
7. The method for preparing the aldehyde-modified silicone oil according to claim 1, characterized in that: The catalyst in step 1) is PT-5000YB catalyst produced by Guangzhou Siyou New Material Technology Co., Ltd.
8. Aldehyde-modified silicone oil prepared by the method for preparing aldehyde-modified silicone oil according to any one of claims 1 to 7.
9. Use of the aldehyde-modified silicone oil according to claim 8 in preparing a hydrophobic coating, characterized in that: The method for preparing the hydrophobic coating comprises the following steps: S1 is respectively prepared with ethyl acetate solution of aldehyde-modified silicone oil and diethylenetriamine; S2: spraying the ethyl acetate solution of aldehyde-modified silicone oil and the ethyl acetate solution of diethylenetriamine on the surface of the glass sheet in sequence, placing it at 25-30° C. until the surface liquid solidifies, thereby obtaining the hydrophobic coating material.
10. Use of the aldehyde-modified silicone oil according to claim 9 in preparing a hydrophobic coating, characterized in that: In step S1, the mass concentration of the aldehyde-modified silicone oil is 50-55%, and the mass concentration of diethylenetriamine is 50-55%.
Citation Information
Patent Citations
Preparation method for branched silane and polyether alkyl co-modified silicone oil
CN109796597A
Preparation method of long-chain alkyl phenyl modified silicone oil
CN111333845A
Phenolic resin modified silicone rubber ablation-resistant coating material as well as preparation method and application thereof
CN116462975A
Organic silicon emulsifier as well as preparation method and application thereof
CN117659410A
Aromatic silicone oil with reaction activity, preparation method and application
CN118085301A
Cited By
Underwater-curable organic silica gel as well as preparation method and application thereof
CN121427097A