Mixed conductive hydrogel, preparation method and application of mixed conductive hydrogel in preparation of wearable electrical stimulation antibacterial patch battery
By using Pam/Imd/PSS:PEDOT hybrid conductive hydrogel and coupled battery electrical stimulation antibacterial device, the problems of high impedance, poor adhesion and mechanical mismatch of traditional electrical stimulation technology in diabetic wound healing have been achieved. Efficient bacterial sterilization and biofilm inhibition, promoting wound healing.
Patent Information
- Application Number
- CN202410742580.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Traditional electrical stimulation antibacterial technology has high impedance, poor adhesion and mechanical mismatch in diabetic wound healing, resulting in limited antibacterial effect and difficulty in inhibiting bacterial resistance and biofilm formation.
It uses a Pam/Imd/PSS:PEDOT hybrid conductive hydrogel composed of acrylamide monomer, imidazolium salt monomer and conductive polymer PSS:PEDOT, combined with a coupled battery electrical stimulation antibacterial device, using oxygen charging and electrochemical reactions to generate microorganisms. current, disrupting bacterial membrane potential and inhibiting biofilm formation.
A hydrogel with low impedance, high adhesion and high conductivity is achieved to ensure the accuracy and stability of signal transmission, effectively sterilize and inhibit the formation of biofilm, reduce wound infection, and reduce the production of TNF-α and IL-6 Expression to promote wound healing.
Smart Images

Figure CN118772441A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional polymer materials, and specifically relates to a mixed conductive hydrogel with low impedance and high adhesion, a preparation method and an application thereof in preparing a wearable electric stimulation antibacterial patch battery. Background Art
[0002] Wound healing is a complex and strictly regulated physiological process, including four overlapping and independent stages coordinated by cellular and humoral factors, namely hemostasis, inflammation, proliferation and remodeling. Bacterial infection is the main reason for hindering wound healing, especially chronic wounds. Compared with normal wounds, chronic wounds stagnate in the inflammatory stage for a long time, making it difficult to heal in an orderly and timely manner and accompanied by persistent infection. As a typical chronic wound, one of the main reasons for the chronicity and difficulty in healing of diabetic wounds is wound infection. Because the blood sugar level in diabetic wounds is high, it is very conducive to the growth and reproduction of pathogens, and eventually a biofilm is formed at the wound, resulting in aggravated wound infection, prolonged inflammation and delayed wound healing. The traditional treatment for bacterial infection is the use of antibiotics, but the abuse of antibiotics can lead to bacterial resistance. In addition, the formation of biofilms is another important cause of drug resistance. Biofilms can prevent the invasion of immune cells and antibiotics through chemical signal communication and DNA sharing mechanisms in quorum sensing, enhance resistance to the outside, and protect bacteria from being killed. More importantly, the enhanced bacterial resistance makes the bacterial biofilm always exist on the wound surface, making it impossible to carry out the next step of treatment. Therefore, combating bacterial infection and inhibiting the growth of biofilm are crucial for treating diabetic wounds.
[0003] In recent years, adjuvant treatments such as wound dressings, oxygen therapy, tissue engineering and electrical stimulation have been proven to be effective in killing bacteria, shortening the inflammatory period and promoting the healing of diabetic wounds. Among them, electrical stimulation (ES) antibacterial technology is an effective method that uses electric current to inhibit and kill bacteria and other microorganisms. It has been widely used in medical, food processing, water treatment and other fields. Electrical stimulation can inhibit the activity of wound bacteria without causing allergic reactions or the production of antibiotic-related resistant bacteria. At present, the antibacterial mechanism based on electrical stimulation mainly includes destroying the potential balance of bacterial cell membranes, increasing membrane permeability, interfering with bacterial electron transfer and increasing the generation of reactive oxygen species (ROS). Electroactive materials can simulate the electrical microenvironment of bone tissue through self-promoting electrochemical reactions, thereby inhibiting bacterial adhesion and proliferation. In addition, applying external current to electroactive materials can interfere with electron transfer in bacteria, induce ROS bursts in bacteria, lead to bacterial death, and inhibit the formation of biofilms. However, due to the specific microenvironment of the wound bed, especially the high level of glutathione (GSH) in the biofilm, the generated ROS may be consumed, thereby compromising the antibacterial effect. In addition, the mechanical mismatch between traditional metal electrodes and biological tissues makes it difficult for them to adapt to the complex wound environment, thereby reducing the stimulation efficiency. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a hybrid conductive hydrogel with low impedance and high adhesion and its application in preparing a coupled battery electric stimulation antibacterial device and a wearable electric stimulation antibacterial patch battery. The hybrid conductive hydrogel is a Pam / Imd / PSS:PEDOT (PIT) hybrid conductive hydrogel composed of acrylamide monomer, imidazole salt monomer and conductive polymer PSS:PEDOT. Due to its good adhesion to tissue (100kPa, such as Figure 4 As shown), low interface impedance (10 3 Ω, such as Figure 3 ) and high conductivity (300mS / cm, as Figure 2As shown), it can establish good conformal contact with the skin, ensuring the accuracy and stability of the two-way signal transmission between the two. In particular, when the conductive hydrogel is used to prepare a coupled battery (CB) electrically stimulated antibacterial device, the device can be quickly charged using oxygen in the air, and the products of the electrochemical reaction and the generated microcurrent during discharge can effectively sterilize Escherichia coli and Staphylococcus aureus, while inhibiting the formation of biofilm. The experimental results show that the device destroys the membrane potential of bacteria and damages the bacterial membrane through positively charged electrodes and ROS and zinc ions generated by electrochemical reactions. At the same time, the microcurrent generated by the electrochemical reaction interferes with the electron transfer in the bacteria, increases the production of ROS in the bacteria, causes oxidative damage to the bacteria, leads to cytoplasm leakage, inhibits the formation of biofilm, reduces wound infection, and reduces the expression of tumor necrosis factor α (TNF-α) and interleukin-6 (IL-6). This work provides a strategy for realizing an integrated wearable electrically stimulated patch battery for wearable and antibacterial treatment.
[0005] The preparation steps of the hydrogel and wearable electrical stimulation patch battery of the present invention are as follows:
[0006] (1) Preparation of Pam / Imd / PSS:PEDOT (PIT) hybrid conductive hydrogel
[0007] ① Add 0.01-0.02 g of conductive polymer poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS) into 1 mL of deionized water, and prepare a PEDOT:PSS aqueous dispersion by a low-temperature ultrasonic method;
[0008] ② Add 0.2-0.6 g of acrylamide (AM), 0.2-0.5 g of 1-butyl-3-vinyl imidazole bromide (IMD) and 0.001-0.003 g of N,N′-methylenebis(2-acrylamide) (MBA) to the PEDOT:PSS aqueous dispersion prepared in step ① and stir evenly, and remove oxygen in the precursor solution by nitrogen bubbling;
[0009] ③ Add 0.01-0.03 g of ammonium persulfate (APS) to the solution obtained in step ②, mix well, and initiate free radical polymerization;
[0010] ④ Add 20-40 μL of N,N,N,N′-tetramethylethylenediamine solution to the solution obtained in step ③, mix thoroughly, pour into a polytetrafluoroethylene mold, and let stand at room temperature for 0.5-2.0 hours to ensure that the monomer can completely undergo polymerization reaction to obtain Pam / Imd / PSS:PEDOT (PIT) mixed conductive hydrogel, i.e., PIT mixed conductive hydrogel;
[0011] (2) Preparation of polyacrylamide (PAM) hydrogel
[0012] 0.2-0.4 g of acrylamide (AM) is added to 1 mL of deionized water, and after fully dissolving, 0.001-0.003 g of N,N′-methylenebis(2-acrylamide) (MBA) and 0.01-0.03 g of ammonium persulfate (APS) are added, and free radical polymerization is initiated by stirring. After stirring evenly, 20-40 μL of N,N,N,N′-tetramethylethylenediamine solution is added, and after fully mixing evenly, the mixture is poured into a polytetrafluoroethylene mold and allowed to stand at room temperature for 0.5-2.0 hours to ensure that the monomer can completely undergo polymerization reaction, thereby obtaining polyacrylamide (PAM) hydrogel, i.e., PAM hydrogel;
[0013] (3) Preparation of Pam / Imd(PI2) hydrogel
[0014] 0.2-0.4 g of acrylamide (AM), 0.3-0.5 g of 1-butyl-3-vinyl imidazole bromide (IMD) and 0.001-0.003 g of N,N′-methylenebis(2-acrylamide) (MBA) were added to 1 mL of deionized water, and then 0.01-0.03 g of ammonium persulfate (APS) was added after fully dissolving, and free radical polymerization was initiated by stirring. After stirring evenly, 20-40 μL of N,N,N,N′-tetramethylethylenediamine solution was added, and after fully mixing evenly, the mixture was poured into a polytetrafluoroethylene mold and allowed to stand at room temperature for 0.5-2.0 hours to obtain Pam / Imd (PI2) hydrogel, i.e., PI2 hydrogel;
[0015] (4) Preparation of polyvinyl alcohol / phosphate buffered saline (PVA / PBS) solid electrolyte
[0016] 3-5 g of polyvinyl alcohol (PVA) is added to 50 mL of a 0.01 M phosphate buffered saline (PBS) solution, and the solution is continuously stirred in an oil bath at 85-95° C., and after being fully dissolved and cooled to room temperature, the solution is added to a polytetrafluoroethylene mold, and then frozen at -30--20° C. for 4-6 hours, and then thawed at room temperature for 30-50 minutes; the "freezing-room temperature thawing" operation is repeated 4-6 times, and after the last thawing, a flexible polyvinyl alcohol / phosphate buffered saline (PVA / PBS) solid electrolyte, i.e., a PVA / PBS solid electrolyte, is obtained, with a thickness of 0.6-0.8 mm;
[0017] (5) Preparation of coupled battery (CB) electrical stimulation antibacterial device
[0018] Since the PIT hybrid conductive hydrogel has adhesive properties, it was adhered to the inner wall of the culture dish, and the zinc strip was fixed to the inner wall of the culture dish on the other side of the PIT hybrid conductive hydrogel. The pins of the 2-5 kΩ color ring resistor were inserted into the PIT hybrid conductive hydrogel and the zinc strip, respectively, to contain 10 3 ~10 4 The nutrient broth medium of CFU / mL of Escherichia coli or Staphylococcus aureus bacterial solution is used as electrolyte to form a complete circuit, that is, a coupled battery (CB) electric stimulation antibacterial device, namely, a CB electric stimulation device;
[0019] (6) Preparation of wearable electrical stimulation patch battery
[0020] The PVA / PBS solid electrolyte (2x3 cm) prepared in step (4) is pasted onto the surface of 3M medical tape (3x4 cm), and then a zinc strip (0.5x2 cm) and a stainless steel sheet (2x2 cm) are placed parallel to each other and independently on the PVA / PBS solid electrolyte, and a PIT mixed conductive hydrogel (1.5x1.5 cm) is placed on the stainless steel sheet, and then the two ends of a 4-6 kΩ color ring resistor are connected to the zinc strip and the PIT mixed conductive hydrogel respectively through copper tape, thereby obtaining the wearable electrical stimulation antibacterial patch battery described in the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 : Fourier transform infrared spectra of PAM, PI2 and PIT2 hydrogels synthesized by the present invention;
[0022] Figure 2 : Conductivity bar graph of PI2, PIT1, PIT2 and PIT3 hydrogels synthesized by the present invention;
[0023] Figure 3 : Epidermal impedance test spectra of PI2, PIT1, PIT2 and PIT3 hydrogels synthesized by the present invention;
[0024] Figure 4 : Column chart of the adhesion of the PIT2 hybrid conductive hydrogel synthesized by the present invention to different materials;
[0025] Figure 5 : The biocompatibility bar graph of the PIT2 hybrid conductive hydrogel synthesized by the present invention when the extract concentration is 0.02g / mL, 0.04g / mL, 0.06g / mL, 0.08g / mL, and 0.1g / mL and co-cultured with mouse embryonic fibroblasts NIH3T3 for 3 days;
[0026] Figure 6 : Cyclic voltammetry curves of the PIT2 hybrid conductive hydrogel synthesized in the present invention at different scan rates;
[0027] Figure 7 : The discharge curve diagram of the electric stimulation antibacterial device prepared by the present invention when different external resistors are connected;
[0028] Figure 8 : A graph showing the voltage variation over time of the electric stimulation antibacterial device prepared by the present invention during air self-charging-electrochemical discharge;
[0029] Fig. 9 After chemical charging for 12 hours, the electric stimulation antibacterial device prepared by the present invention has a high conductivity at 5-100 μA cm -2 Changes in current density during electrochemical discharge for 1 h;
[0030] Fig.10 : Bacterial activity diagram of the PIT2 hybrid conductive hydrogel, UB and CB electric stimulation antibacterial device prepared by the present invention after co-culture with Escherichia coli for 24 hours;
[0031] Fig.11 : Bacterial activity diagram of the PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation antibacterial device prepared by the present invention after co-culture with Staphylococcus aureus for 24 hours;
[0032] Fig.12 : Biofilm removal rate diagram of the PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation antibacterial devices prepared by the present invention after co-culture with Escherichia coli biofilm for 24 hours;
[0033] Fig.13 : Biofilm clearance rate diagram of the PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation antibacterial devices prepared by the present invention after co-culture with Staphylococcus aureus biofilm for 24 hours;
[0034] Fig.14 : A graph showing the change in ROS fluorescence intensity over time when the UB and CB electrical stimulation antibacterial devices prepared by the present invention are added / not added with 8 mM glutathione (GSH) in nutrient broth medium;
[0035] Fig.15 : A graph showing the change of glutathione consumed by the UB and CB electrical stimulation antibacterial devices prepared by the present invention in nutrient broth medium over time;
[0036] Fig.16 : Bar graph of glutathione content in biofilm after co-culture of PIT2 hybrid conductive hydrogel, UB and CB electric stimulation antibacterial devices prepared by the present invention with Staphylococcus aureus biofilm for 24 hours;
[0037] Fig.17: Quantitative bar graph of nucleic acid leakage in bacteria after co-culture of PIT2 hybrid conductive hydrogel, UB and CB electric stimulation antibacterial devices prepared by the present invention with Escherichia coli and Staphylococcus aureus for 24 hours;
[0038] Fig.18 : The quantitative bar graph of protein leakage in bacteria after co-culture of PIT2 hybrid conductive hydrogel, UB and CB electric stimulation antibacterial devices with Escherichia coli for 24 hours;
[0039] Fig.19 : Quantitative bar graph of protein leakage in bacteria after co-culture of PIT2 hybrid conductive hydrogel, UB and CB electric stimulation antibacterial devices prepared by the present invention with Staphylococcus aureus for 24 hours;
[0040] Fig. 20 : The bar graph of zinc ion concentration in the culture medium after the UB and CB electric stimulation antibacterial devices prepared by the present invention were discharged in the nutrient broth culture medium for 24 hours;
[0041] Fig.21 : Schematic diagram of the structure of the CB electric stimulation antibacterial device prepared by the present invention;
[0042] Fig. 22 : Schematic diagram of the wearable electrical stimulation antibacterial patch battery prepared by the present invention.
[0043] like Figure 1 As shown in the figure, the Fourier transform infrared spectra of PAM, PI2, and PIT2 hybrid conductive hydrogels were tested using a Fourier transform infrared spectrometer, in which the amino and carbonyl absorption peaks of acrylamide are located at 3340 cm -1 and 1670cm -1 , CN of imidazolium salt + The absorption peak is located at 1325 cm -1 The characteristic peak of PEDOT:PSS is located at 1016cm -1 (-SO3 -) and 1127, 1083cm -1 (CO).
[0044] like Figure 2 As shown in the figure, different quantities of AM and IMD (MR) were tested using a source meter and a four-point probe. AM / IMD=1.2), wherein the content of AM in PIT1 is 0.28g and the content of IMD is 0.23g; the content of AM in PIT2, i.e. the hydrogel prepared by the present invention, is 0.4g and the content of IMD is 0.33g; the content of AM in PIT3 is 0.55g and the content of IMD is 0.42g; the PI2 hydrogel does not contain the conductive polymer PEDOT:PSS, and the contents of all other components are the same as those of the PIT2 conductive hydrogel. As can be seen from the figure, the conductivity of the PIT2 conductive hydrogel prepared in Example 1 of the present invention is 33.2S m -1 , which is significantly higher than that of the other three hydrogels.
[0045] like Figure 3 As shown in the figure, the epidermal impedance of PI2, PIT1, PIT2, and PIT3 hydrogels was tested using an electrochemical workstation. A dual-electrode system was used for epidermal impedance testing. The hydrogel (8 mm in diameter, 1 mm in thickness) was used as the working electrode and the counter electrode. The two circular electrodes were attached to the skin surface of the forearm in parallel (center distance 2 cm) at a scanning frequency of 10 6 ~10 0 It can be seen that PIT2 conductive hydrogel exhibits low interfacial impedance at both high and low frequencies, among which the interfacial impedance of PIT2 conductive hydrogel at 1 Hz is 1.04 kΩ. Since PIT2 conductive hydrogel has high conductivity and low epidermal impedance, PIT2 conductive hydrogel is used in all subsequent experiments.
[0046] like Figure 4 As shown, the PIT2 hybrid conductive hydrogel was sandwiched between two pieces of pigskin / glass / metal, and the adhesion properties of the PIT2 hybrid conductive hydrogel to various substrates were tested by stretching the pigskin / glass / metal at a rate of 20 mm / min using a universal testing machine. The adhesion strength of the hydrogel to different materials was quantitatively characterized, and the adhesion strength to pigskin could reach 56 kPa. This interfacial adhesion was attributed to the multiple dynamic non-covalent interactions between the amino groups and cations in the PIT2 hybrid conductive hydrogel and the active groups on the tissue surface, including hydrogen bonding, dipole-dipole interactions, and electrostatic attraction.
[0047] like Figure 5As shown, the cytotoxicity of different concentrations of PIT2 hybrid conductive hydrogel extracts on mouse fibroblasts NIH3T3 fibroblasts was evaluated by MTT test. The prepared PIT2 hybrid conductive hydrogel was placed in DMEM culture medium for extraction, and the extract was diluted with culture medium in proportion to obtain hydrogel extracts with concentrations of 0.02g / mL, 0.04g / mL, 0.06g / mL, 0.08g / mL, and 0.1g / mL. Although the cell survival rate decreased slightly with the increase in the concentration of PIT2 hybrid conductive hydrogel extract, the overall cell survival rate was always greater than 90%, indicating that the toxicity of PIT2 conductive hydrogel was low.
[0048] like Figure 6 As shown in the figure, the cyclic voltammetry (CV) curves of PIT2 hybrid conductive hydrogel at different scan rates (2-10mV / s) were measured by an electrochemical workstation. In a three-electrode system, PIT2 hybrid conductive hydrogel was used as the working electrode, Ag / AgCl electrode was used as the reference electrode, platinum electrode was used as the counter electrode, and 0.1M phosphate buffer solution was used as the electrolyte solution. The cyclic voltammetry curves of PIT2 hybrid conductive hydrogel at scan rates of 2mV / s, 4mV / s, 6mV / s, 8mV / s, and 10mV / s were tested by an electrochemical workstation. It can be seen from the curve that the CV curve of PIT2 hybrid conductive hydrogel has a redox peak at -0.4 / -0.1V (Ag / AgCl), which is attributed to the doping and dedoping process of PEDOT. And the CV curves show similar shapes, the current intensity of the peak current increases with the continuous increase of the scan rate, and shows a high degree of symmetry, indicating that PIT2 hybrid conductive hydrogel has fast discharge / charge dynamics.
[0049] like Figure 7 As shown, the discharge curve of the electric stimulation antibacterial device prepared by the present invention when connected to different external resistors (1 to 10 kΩ) was tested on a Newell battery testing machine, demonstrating the actual long-term electrochemical discharge-chemical charging process, wherein the discharge curve shows that the midpoint discharge voltage is 0.38 V, and when the resistance is 5 kΩ, the discharge time is as long as 200 hours.
[0050] like Figure 8 As shown in the figure, the electric stimulation antibacterial device prepared by the present invention was tested on a Newell battery tester during the air self-charging process. The battery was charged at 100 μA cm in the air environment. -2 After discharging to 0.3V at a current density, the battery was exposed to the air, allowing the oxygen in the air to react with the PIT2 mixed conductive hydrogel cathode to undergo an air self-charging process. It took only 60 minutes for the battery to reach 1.0V (97% of the initial OCV level), demonstrating the battery's rapid self-charging process.
[0051] like Fig. 9 As shown, the electric stimulation antibacterial device prepared by the present invention was chemically charged for 12 hours on a Newell battery tester and charged at 5 to 100 μA cm -2 The electrochemical discharge capacity of the battery was studied at a current density of 5 to 100 μA cm for 1 h. -2 The battery was electrochemically discharged at a rate of 2.5 % and charged with oxygen when exposed to air, indicating that the battery has good recovery ability.
[0052] like Fig.10 As shown, the optical density values at 600nm of CTR, PIT2, UB and CB electric stimulation antibacterial devices and Escherichia coli were measured by UV-visible spectrophotometer after co-culture with Escherichia coli for 24 hours at 37°C. Among them, CTR is the control group, which only has Escherichia coli culture medium; PIT2 is the gel group, and PIT2 mixed conductive hydrogel is placed on one side of the Escherichia coli culture medium; UB is the uncoupled battery group, and zinc strips and PIT2 mixed conductive hydrogel are placed on both sides of the Escherichia coli culture medium; CB is the coupled battery group, that is, the electric stimulation antibacterial device group prepared by the present invention, which connects the zinc strips and PIT2 mixed conductive hydrogel through a 5kΩ resistor on the basis of the UB group, and forms a complete circuit with the culture medium for electrical stimulation. The initial concentration of Escherichia coli is 10 4 CFU / mL (colony forming unit, CFU), after 24 hours of co-culture, the number of bacteria in the CTR group increased significantly, and the optical density of bacteria at 600nm exceeded 1.6. The optical density of the bacterial solution treated with PIT2 conductive hydrogel, UB and CB groups decreased significantly, indicating a decrease in the number of bacteria. It is worth noting that the antibacterial rate of UB against Escherichia coli was 66%, which was always higher than that of PIT2 conductive hydrogel (the antibacterial rate against Escherichia coli was 57%), and the antibacterial rate of CB group against Escherichia coli was 87%.
[0053] like Fig.11 As shown, the optical density values at 600nm of CTR, PIT2, UB and CB electric stimulation antibacterial devices and Staphylococcus aureus were measured by UV-visible spectrophotometer after co-culture at 37°C for 24 hours. Among them, CTR is the control group, which only has Staphylococcus aureus culture medium; PIT2 is the gel group, and PIT2 mixed conductive hydrogel is placed on one side of the Staphylococcus aureus culture medium; UB is an uncoupled battery group, and zinc strips and PIT2 mixed conductive hydrogel are placed on both sides of the Staphylococcus aureus culture medium; CB is a coupled battery group, that is, the electric stimulation antibacterial device group prepared by the present invention, which is based on the UB group, and the zinc strips and PIT2 mixed conductive hydrogel are connected through a 5kΩ resistor, and form a complete circuit with the culture medium for electrical stimulation. The initial concentration of Staphylococcus aureus is 10 4CFU / mL (colony forming unit, CFU), after 24 hours of co-culture, the number of bacteria in the CTR group increased significantly, and the optical density of bacteria at 600nm exceeded 1.4. The optical density of the bacterial solution treated with PIT2 conductive hydrogel, UB and CB groups decreased significantly, indicating a decrease in the number of bacteria. It is worth noting that the antibacterial rate of UB against Escherichia coli was 65%, which was always higher than that of PIT2 conductive hydrogel (the antibacterial rate against Escherichia coli was 59%), and the antibacterial rate of CB group against Staphylococcus aureus was 83%.
[0054] like Fig.12 As shown in the figure, the biofilm removal rates of CTR, PIT2, UB and CB electric stimulation antibacterial devices after co-culture with E. coli biofilm for 24 hours were tested to evaluate the inhibitory ability of CB electric stimulation antibacterial device on E. coli biofilm formation. 3 mL (10 8 CFU / mL), covered with a round glass cover and cultured in an incubator at 37°C for 48 hours to obtain E. coli biofilm. Then the culture medium was treated with CTR, PIT2, UB, and CB for 24 hours. After different treatments, it was washed with PBS three times, incubated with anhydrous methanol for 10 minutes, stained with 500μL crystal violet (1g / L) for 10 minutes, washed with PBS three times, air-dried and photographed, and the stained biofilm was dissolved in 500μL 95% ethanol, and the absorbance at 570nm was measured with an enzyme reader. The normalized crystal violet absorbance value quantification showed that the inhibition rate of CB on E. coli biofilm was 82%, indicating that CB can effectively fight E. coli, further deconstruct biofilm, eliminate bacterial infection barriers in chronic wound healing, and shorten healing time.
[0055] like Fig.13 As shown in the figure, the biofilm removal rates of CTR, PIT2, UB and CB electrical stimulation antibacterial devices after co-culture with Staphylococcus aureus biofilm for 24 hours were tested to evaluate the inhibitory ability of CB electrical stimulation antibacterial device on the biofilm formation of Staphylococcus aureus. 3 mL (10 8CFU / mL), covered with a round glass cover and cultured in an incubator at 37°C for 48 hours to obtain Staphylococcus aureus biofilm. The culture medium was then treated with CTR, PIT2, UB, and CB for 24 hours. After different treatments, it was washed 3 times with PBS, incubated with anhydrous methanol for 10 minutes, stained with 500μL crystal violet (1g / L) for 10 minutes, washed 3 times with PBS, air-dried and photographed, and the stained biofilm was dissolved in 500μL 95% ethanol, and the absorbance at 570nm was measured with an enzyme reader. The normalized crystal violet absorbance value quantification showed that the inhibition rate of CB on Staphylococcus aureus biofilm was 84%, indicating that CB can effectively fight Staphylococcus aureus, further deconstruct biofilms, eliminate bacterial infection barriers in chronic wound healing, and shorten healing time.
[0056] like Fig.14 As shown, considering that the electrochemical discharge process can produce low concentrations of free radicals, we used 2',7'-dichlorodihydrofluorescein (DCFH-DA) fluorescent probe to monitor the ROS level in the nutrient broth medium. The UB and CB electrical stimulation antibacterial devices prepared by the present invention were incubated in nutrient broth medium for 3 hours, and the ROS generated by the CB group in the nutrient broth medium was 9.2 times that of the UB group. In addition, when the UB and CB electrical stimulation antibacterial devices prepared by the present invention were added to the nutrient broth medium with 8mM glutathione (GSH) similar to the content in the biofilm and incubated for 3 hours, the ROS level in the nutrient broth medium of the UB group decreased slightly due to the consumption of GSH. In contrast, when the GSH content in the nutrient broth medium was low (40% of the initial level), the ROS level of the CB group decreased by 46%.
[0057] like Fig.15 As shown, the UB and CB electric stimulation antibacterial devices prepared by the present invention were tested for their consumption of glutathione (GSH) in nutrient broth medium. 18 g of nutrient broth dry powder medium (10 g of peptone, 3 g of beef extract powder, 5 g of sodium chloride) was weighed and dissolved in 1000 mL of purified water, heated and dissolved, and then autoclaved at 121°C for 15 minutes to prepare the required nutrient broth medium. Within 3 hours, the GSH content in the nutrient broth medium of the UB group remained at 90% of the initial level. In contrast, the GSH content in the nutrient broth medium of the CB group was only 40% left.
[0058] like Fig.16 To investigate whether the CB electrical stimulation antibacterial device can decompose glutathione (GSH) in the Staphylococcus aureus biofilm, the prepared PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation antibacterial devices were tested with 10 8CFU / mL of GSH concentration after 24h of co-culture of Staphylococcus aureus biofilm. After 24h of co-culture, the supernatant was collected by centrifugation, 5μL of 5,5'-dithiobis(2-nitrobenzoic acid) (DTNB) was added to the collected supernatant, incubated in an incubator at 37°C for 30min, and GSH consumption was measured using a 412nm UV-visible spectrophotometer. Compared with the control group, the CB group can significantly reduce the GSH level in the biofilm (reduced to 11% of the initial value).
[0059] like Fig.17 As shown in the figure, in order to evaluate the antibacterial effect of PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation devices, their effects on bacterial nucleic acid leakage after 24 hours of co-culture with Escherichia coli and Staphylococcus aureus were determined. After incubation of CTR, PIT2, UB and CB groups with Escherichia coli and Staphylococcus aureus at 37°C for 24 hours, they were filtered with a 0.22μm syringe filter membrane, and the filtrate aliquots (200μL) were added to 96-well plates. The absorbance value (OD260 value) at 260nm was measured by a microplate reader to evaluate the presence of nucleic acids. By comparing the amount of bacterial nucleic acid leakage between different treatment groups and the control group, it can be seen that the leakage of the CB group was significantly higher than that of the control group, indicating that the treatment method has a stronger destructive effect on the bacterial cell membrane.
[0060] like Fig.18 As shown, the effects of the PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation devices prepared by the present invention on the protein leakage of Escherichia coli after 24 hours of co-culture were evaluated. The release of proteins in Escherichia coli cells was determined by colorimetry using a commercial kit (enhanced biuret acid (BCA) protein assay kit). After the Escherichia coli cells were incubated at 37°C for 24 hours in a nutrient broth medium, the cells were collected, centrifuged (4000rpm, 5min), and washed three times with phosphate buffered saline (PBS). The Escherichia coli suspension was treated with CTR, PIT2, UB and CB at 37°C for 24 hours, and the supernatant was collected by centrifugation. 200μL of BCA working solution was added to the collected supernatant. The samples were incubated at 37°C for 30 minutes, and the absorbance was measured using a microplate reader. Under the same reaction conditions and procedures, a standard curve was prepared. According to the bar graph, the protein leakage in the CB group was significantly higher than that in the control group, indicating that the treatment method had a stronger destructive effect on the Escherichia coli cell membrane.
[0061] like Fig.19As shown, the effects of the PIT2 hybrid conductive hydrogel, UB and CB electrical stimulation devices prepared by the present invention on the protein leakage of Staphylococcus aureus after 24 hours of co-culture were evaluated. The release of proteins in Escherichia coli cells was determined by colorimetry using a commercial kit (enhanced biuret acid (BCA) protein assay kit). Staphylococcus aureus cells were incubated in nutrient broth medium at 37°C for 24 hours, and the cells were collected by centrifugation (4000rpm, 5min), and washed three times with phosphate buffered saline (PBS). Staphylococcus aureus suspension was treated with CTR, PIT2, UB and CB at 37°C for 24 hours, and the supernatant was collected by centrifugation. 200μL of BCA working solution was added to the collected supernatant. The samples were incubated at 37°C for 30 minutes, and the absorbance was measured using a microplate reader. Under the same reaction conditions and procedures, a standard curve was prepared. According to the bar graph, the protein leakage in the CB group was significantly higher than that in the control group, indicating that the treatment method had a stronger destructive effect on the cell membrane of Staphylococcus aureus.
[0062] like Fig. 20 As shown, the changes in zinc ion (Zn2+) concentration in the nutrient broth medium after 24 h of discharge of UB and CB electrical stimulation devices were evaluated. After 24 h, the concentration of soluble Zn2+ in the UB medium increased. 2+ Concentration: 43.5 μg mL -1 , while Zn in CB 2+ The concentration is 4.3 times that of UB, which significantly increases the Zn content in the culture medium. 2+ concentration.
[0063] like Fig.21 As shown, it is a structural demonstration diagram of the CB electric stimulation antibacterial device prepared by the present invention. Since the PIT2 mixed conductive hydrogel has adhesion, it is adhered to the side wall of the culture dish, the zinc strip is fixed on the opposite side of the PIT2 mixed conductive hydrogel, and the pins of the 5kΩ color ring resistor are mixed with the conductive hydrogel to obtain the wearable electric stimulation antibacterial patch battery described in the present invention. DETAILED DESCRIPTION
[0064] Example 1
[0065] (1) Preparation of Pam / Imd / PSS:PEDOT(PIT2) hybrid conductive hydrogel:
[0066] ① Add 0.015 g of conductive polymer poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS) into 1 mL of deionized water and prepare a PEDOT:PSS aqueous dispersion (concentration 1.5 wt%) by low-temperature ultrasonic method;
[0067] ② Add 0.4 g of acrylamide (AM), 0.33 g of 1-butyl-3-vinylimidazolium bromide (IMD) and 0.002 g of N,N′-methylenebis(2-acrylamide) (MBA) to the PEDOT:PSS aqueous dispersion prepared in step ①, stir evenly, and remove oxygen from the precursor solution by nitrogen bubbling;
[0068] ③ Add 0.02 g of ammonium persulfate (APS) to the solution obtained in step ② and mix well to initiate free radical polymerization;
[0069] ④ Add 30 μL of N,N,N,N′-tetramethylethylenediamine solution to the solution obtained in step ③, mix thoroughly, pour into a polytetrafluoroethylene mold, and let stand at room temperature for 1 hour to ensure that the monomer can completely undergo polymerization reaction; obtain Pam / Imd / PSS:PEDOT (PIT2) hybrid conductive hydrogel, i.e., PIT2 hybrid conductive hydrogel;
[0070] (2) Preparation of polyacrylamide (PAM) hydrogel
[0071] 0.4 g of acrylamide (AM) was added to 1 mL of deionized water. After fully dissolving, 0.002 g of N,N′-methylenebis(2-acrylamide) (MBA) and 0.02 g of ammonium persulfate (APS) were added. Free radical polymerization was initiated by stirring. After stirring evenly, 30 μL of N,N,N,N′-tetramethylethylenediamine solution was added. After fully mixing, the mixture was poured into a polytetrafluoroethylene mold and allowed to stand at room temperature for 1 hour to ensure that the monomers could completely undergo polymerization reaction to obtain PAM hydrogel.
[0072] (3) Preparation of Pam / Imd(PI2) hydrogel
[0073] 0.4 g of acrylamide (AM), 0.33 g of 1-butyl-3-vinylimidazolium bromide (IMD) and 0.002 g of N,N′-methylenebis(2-acrylamide) (MBA) were added to 1 mL of deionized water, and then 0.02 g of ammonium persulfate (APS) was added to fully dissolve them. Free radical polymerization was initiated by stirring, and 30 μL of N,N,N,N′-tetramethylethylenediamine solution was added after stirring. After fully mixing, the mixture was poured into a polytetrafluoroethylene mold and allowed to stand at room temperature for 1 hour to ensure that the monomers could completely undergo polymerization reaction, thereby obtaining PI2 hydrogel.
[0074] (4) Preparation of polyvinyl alcohol / phosphate buffered saline (PVA / PBS) solid electrolyte:
[0075] 4.5 g of polyvinyl alcohol (PVA) was added to 0.01 M phosphate buffered saline (PBS) solution (50 mL), and the solution was stirred continuously in a 90 ° C oil bath. After it was fully dissolved and cooled to room temperature, the solution was added to a polytetrafluoroethylene mold, which was then frozen at -25 ° C for 5 hours and thawed at room temperature for 40 minutes; the "freeze-room temperature thawing" operation was repeated 5 times, and a flexible PVA / PBS solid electrolyte with a thickness of 0.7 mm was obtained after the last thawing. (5) Preparation of coupled battery (CB) electrical stimulation antibacterial device:
[0076] Since the PAM / IMD / PSS:PEDOT hybrid conductive hydrogel (PIT2) has adhesive properties, it was adhered to the inner wall of the culture dish, and the zinc strip was fixed to the inner wall of the culture dish on the other side of the PIT2 hybrid conductive hydrogel. The pins of the 5kΩ color ring resistor were inserted into the PIT2 hybrid conductive hydrogel and the zinc strip, respectively, to contain 10 4 The nutrient broth culture medium containing CFU / mL of Escherichia coli or Staphylococcus aureus was used as the electrolyte to form a complete circuit, which was the CB electrical stimulation device used in the test.
[0077] (6) Preparation of wearable electrical stimulation patch battery:
[0078] First, the PVA / PBS solid electrolyte (2x3 cm) prepared in step (2) is pasted onto the surface of 3M medical tape (3x4 cm), and then a zinc strip (0.5x2 cm) and a stainless steel sheet (2x2 cm) are placed parallel to each other and independently on the PVA / PBS solid electrolyte, and a PIT2 mixed conductive hydrogel (1.5x1.5 cm) is placed on the stainless steel sheet, and then the two ends of a 5kΩ color ring resistor are connected to the zinc strip and the PIT2 mixed conductive hydrogel respectively through copper tape, thereby obtaining the wearable electrical stimulation antibacterial patch battery described in the present invention.
Claims
1. A method for preparing a mixed conductive hydrogel, the steps of which are as follows: ① Add 0.01-0.02 g of conductive polymer poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) into 1 mL of deionized water, and prepare a PEDOT:PSS aqueous dispersion by low-temperature ultrasonication; ② Add 0.2-0.6 g of acrylamide, 0.2-0.5 g of 1-butyl-3-vinyl imidazole bromide and 0.001-0.003 g of N,N′-methylenebis(2-acrylamide) to the PEDOT:PSS aqueous dispersion prepared in step ① and stir evenly, and remove oxygen from the precursor solution by nitrogen bubbling; ③ Add 0.01-0.03 g of ammonium persulfate to the solution obtained in step ②, mix well, and initiate free radical polymerization; ④ Add 20-40 μL of N,N,N,N′-tetramethylethylenediamine solution to the solution obtained in step ③, mix thoroughly, pour into a polytetrafluoroethylene mold, and let stand at room temperature for 0.5-2.0 hours to ensure that the monomer can completely undergo polymerization reaction to obtain the Pam / Imd / PSS:PEDOT hybrid conductive hydrogel.
2. A mixed conductive hydrogel, characterized in that: The method is prepared by the method of claim 1.
3. Use of the mixed conductive hydrogel according to claim 2 in preparing a coupled battery electric stimulation antibacterial device.
4. The use of the mixed conductive hydrogel according to claim 3 in preparing a coupled battery electric stimulation antibacterial device, characterized in that: The Pam / Imd / PSS:PEDOT hybrid conductive hydrogel was adhered to the inner wall of the culture dish, the zinc strip was fixed to the inner wall of the culture dish on the other side opposite to the Pam / Imd / PSS:PEDOT hybrid conductive hydrogel, and the pins of the 2-5 kΩ color ring resistor were inserted into the Pam / Imd / PSS:PEDOT hybrid conductive hydrogel and the zinc strip, respectively. 3 ~10 4 The deionized water solution of CFU / mL of Escherichia coli or Staphylococcus aureus is used as electrolyte to form a complete circuit, thus obtaining a coupled battery electrical stimulation antibacterial device.
5. Use of the hybrid conductive hydrogel according to claim 2 in preparing a wearable electrical stimulation antibacterial patch battery.
6. The use of the hybrid conductive hydrogel according to claim 5 in preparing a wearable electrical stimulation antibacterial patch battery, characterized in that: The method is to stick a flexible polyvinyl alcohol / phosphate buffer salt solid electrolyte to the surface of a 3M medical tape, then place a zinc strip and a stainless steel sheet parallel to and independently on the polyvinyl alcohol / phosphate buffer salt solid electrolyte, place a Pam / Imd / PSS:PEDOT mixed conductive hydrogel on the stainless steel sheet, and then connect the zinc strip and the Pam / Imd / PSS:PEDOT mixed conductive hydrogel at both ends of a 4-6 kΩ color ring resistor respectively through a copper tape, thereby obtaining the wearable electrical stimulation antibacterial patch.
7. The use of the hybrid conductive hydrogel according to claim 6 in preparing a wearable electrical stimulation antibacterial patch battery, characterized in that: The method comprises adding 3 to 5 g of polyvinyl alcohol to 50 mL of 0.01 M phosphate buffered saline solution, stirring continuously in an oil bath at 85 to 95° C., adding the solution to a polytetrafluoroethylene mold after it is fully dissolved and cooled to room temperature, and then freezing the mold at -30 to -20° C. for 4 to 6 hours, and then thawing the mold at room temperature for 30 to 50 minutes; The "freeze-room temperature thawing" operation is repeated 4 to 6 times, and after the last thawing, a flexible polyvinyl alcohol / phosphate buffer salt solid electrolyte is obtained with a thickness of 0.6 to 0.8 mm.
Citation Information
Patent Citations
Antibacterial hydrogel material and preparation method and application thereof
CN109503780A
Stretchable transparent conductive hydrogel and preparation method thereof
CN110256694A
Conductive-piezoelectric hydrogel as well as preparation method and application thereof
CN116549676A
Multi-scale pressure sensing hydrogel as well as preparation method and application thereof
CN117024665A
Cited By
Ionic liquid conductive hydrogel as well as preparation method and application thereof
CN120842616A