Propeller preparation material, preparation method thereof and propeller

By using rubber, resin, graphite and other materials to prepare propeller preparation materials, the problems of existing steel propeller blades such as heavy weight, high energy consumption, high noise and easy corrosion are solved, and the propeller is made light in weight, low in energy consumption and self-lubricating. properties and chemical corrosion resistance, which improves the transportation capacity of fine materials and product life.

CN118772497APending Publication Date: 2024-10-15中国化学品安全协会
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010446.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing integral steel propeller blades have problems such as heavy weight, high energy consumption, high noise, and easy corrosion. In particular, they perform poorly in terms of transportation of fine materials and resistance to chemical corrosion.

Method used

Composite materials composed of rubber, resin, graphite, fiber, vulcanizing agent, accelerator, reinforcing agent and plasticizer are used to prepare propeller preparation materials. The propeller is prepared through blending and dipping processes to achieve light weight, low energy consumption, Self-lubricating, low noise and high rigidity.

Benefits of technology

The prepared propeller has light weight, low energy consumption, self-lubrication, low noise, rigidity and excellent chemical corrosion resistance, which improves the transportation capacity of fine materials and product life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964181750000021
    Figure BDA0004964181750000021
  • Figure BDA0004964181750000022
    Figure BDA0004964181750000022
  • Figure BDA0004964181750000031
    Figure BDA0004964181750000031
Patent Text Reader

Abstract

The invention relates to a preparation material for a propeller, a preparation method of the preparation material and the propeller. The preparation material for the propeller comprises reaction products of the following components: rubber, resin, graphite, fibers, a vulcanizing agent, an accelerant, a reinforcing agent and a plasticizer. The propeller material which is light in weight, renewable, low in noise and low in friction lubricity is prepared from the reactants; a propeller prepared from the propeller material has good chemical corrosion resistance and abrasion resistance in a weak acid and weak alkali chemical environment, is a light-weight renewable propeller, and is very suitable for preparing paddles for shaftless screw conveyors for treating solid and liquid for comprehensive utilization of straws and treatment of biogas and sewage. The method disclosed by the invention is novel, simple to prepare, safe, reliable, tough, corrosion-resistant, erosion-resistant and capable of prolonging the service life of the propeller material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conveying equipment, and more particularly to a propeller preparation material and a preparation method thereof. In addition, the present invention also relates to a propeller made from the propeller preparation material. Background Art

[0002] The shaftless screw conveyor is a screw conveyor designed without a center shaft. It uses an integral steel screw with a certain elasticity to push materials. Its main feature is strong anti-winding performance. The design without a center shaft makes the shaftless screw conveyor have special advantages for conveying strip-shaped, viscous materials, and easy-to-wind materials, and can prevent accidents caused by blockage. Good environmental performance, fully enclosed conveying and easy-to-clean spiral surface can ensure environmental hygiene and the conveyed materials are not polluted or leaked. Large torque and low energy consumption. Since the spiral has no shaft, the material is not easy to be blocked and the discharge port is not blocked, so it can run at a lower speed, drive smoothly, and reduce energy consumption. Large conveying capacity, the conveying capacity of the shaftless screw conveyor is 1.5 times that of the traditional shafted screw conveyor of the same diameter. Long conveying distance, the conveying length of a single machine can reach 60 meters, and according to user needs, it can be installed in multi-stage series to convey materials over long distances. Low maintenance cost, the shaftless design reduces maintenance costs and reduces failure rates. High efficiency and energy saving, the use of high-efficiency energy-saving power transmission can reduce energy consumption and maintenance costs, and improve production efficiency. Compact structure, simple design and compact structure allow materials to be transported smoothly in a small space, saving space. The material is easy to clean, and during the conveying process, the material only contacts the shaftless screw, not the shaft, reducing the risk of cross contamination.

[0003] Although the propellers made of steel materials in the prior art have the above advantages, the blades made of them also have some disadvantages. Specifically, the existing integral steel propeller blades have the problems of heavy weight, high energy consumption, high noise, and easy corrosion. In view of this, it has become an urgent problem to be solved by those skilled in the art to develop a propeller preparation material so that the propeller prepared by it has the advantages of light weight, low energy consumption, low noise, and not easy to corrode, and has a good conveying capacity for fine materials. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a propeller preparation material and a preparation method thereof, and a propeller. The propeller preparation material is a composite material composition with light weight, low energy consumption, self-lubrication, low noise, corrosion resistance and rigidity; wherein, the components of the preparation material of the present invention make the propeller made of it have the advantages of light weight and low energy consumption; the self-lubricating property comes from the polymer resin; the low noise comes from the elasticity and resilience of the rubber or thermoplastic rubber, and the rigidity comes from the blending of the fiber and graphite. The propeller preparation material is prepared from the aforementioned multiple materials. The propeller prepared by the propeller preparation material has the advantages of light weight, low energy consumption, self-lubrication, low noise and rigidity; its self-lubrication makes the propeller have better conveying capacity for fine materials, its elasticity and resilience solve the problem of high noise of shaftless screw conveyors in the prior art, realizes shock absorption and noise reduction, and the rigidity of the mixture meets the screw pushing performance. At the same time, the propeller prepared by the propeller preparation material of the present invention also has excellent chemical corrosion resistance and acid and alkali resistance, which can extend the service life of the propeller product.

[0005] One of the purposes of the present invention is to provide a propeller preparation material, wherein the propeller preparation material is prepared by vulcanizing raw materials including the following components: rubber, resin, graphite, fiber, vulcanizing agent, accelerator, reinforcing agent and plasticizer;

[0006] The rubber is calculated by weight as 100 parts:

[0007]

[0008] In a preferred embodiment of the present invention, the rubber is calculated based on 100 parts by weight:

[0009]

[0010]

[0011] In a preferred embodiment of the present invention, the rubber is at least one of chlorinated polyethylene rubber, nitrile rubber, ethylene propylene rubber, and styrene butadiene rubber, preferably carboxylated nitrile rubber, more preferably, the raw rubber Mooney viscosity of the carboxylated nitrile rubber is 60 to 85; and / or, the acrylonitrile content in the carboxylated nitrile rubber is 18 to 45wt%. The technician can select the appropriate specific rubber material, the raw rubber Mooney viscosity of the rubber, and the acrylonitrile content of the rubber according to the actual situation.

[0012] In a preferred embodiment of the present invention, the resin is at least one of polyurethane resin, polyethylene resin, chlorinated polyethylene resin, ultra-high molecular weight polyethylene resin, polypropylene resin, polystyrene resin, polyetherketone resin, polyimide resin, and polyester resin, preferably ultra-high molecular weight polyethylene resin. The "ultra-high molecular weight polyethylene resin" herein may have a molecular weight between 1.2 million and 4 million. The technician may select the appropriate specific resin material and the molecular weight of the resin according to the actual situation.

[0013] In a preferred embodiment of the present invention, the number of layers of the graphene is less than 10, and the graphite is nanographite. It should be noted that the aforementioned graphite can be cryptocrystalline graphite or crystalline graphite. More preferably, the graphite is cryptocrystalline nanographite. Most preferably, the carbon content of the graphite is more than 85%. Technicians can select appropriate graphite or graphene according to actual conditions.

[0014] The fiber may be a natural fiber or a synthetic fiber. In a preferred embodiment of the present invention, the fiber is a short fiber or a mesh fiber, preferably at least one of carbon fiber, aramid fiber, polyester fiber, polyimide fiber, glass fiber, basalt fiber, and synthetic fiber, more preferably a short fiber blended with polyester fiber and aramid fiber (the mass ratio of the two is 1:1). The technician can select the appropriate fiber according to the actual situation.

[0015] In a preferred embodiment of the present invention, the vulcanizing agent is at least one of a peroxide vulcanizing agent, an amine vulcanizing agent, a resin vulcanizing agent, and sulfur. Specifically, the peroxide vulcanizing agent can be selected from at least one of diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, benzoyl peroxide, di-2,4-dichlorobenzoyl peroxide, 1,4-di-tert-butylperoxyisopropylbenzene, and butanediol 2-methacrylate; the amine vulcanizing agent can be selected from hexamethylenediamine carbamate and triethylenetetramine; the resin vulcanizing agent can be selected from at least one of phenolic resin, sulfur-containing alkylphenolic resin, p-tert-butylphenol formaldehyde resin, p-tert-octylphenol formaldehyde resin, and alkylphenol resin. Preferably, the vulcanizing agent is at least one of diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and sulfur. The technician can select a suitable vulcanizing agent according to the actual situation.

[0016] In a preferred embodiment of the present invention, the accelerator is at least one of zinc oxide, magnesium oxide, thiurams, amines, and thiazoles, preferably at least one of N-cyclohexyl-2-benzothiazole sulfenamide and sulfur-containing alkylphenol-formaldehyde resin. The technician can select a suitable accelerator according to the actual situation.

[0017] In a preferred embodiment of the present invention, the reinforcing agent is at least one of carbon black, white carbon black, carbon black, and diatomaceous earth. Preferably, the reinforcing agent is carbon black. The technicians can select a suitable reinforcing agent according to the actual situation.

[0018] In a preferred embodiment of the present invention, the plasticizer is at least one of liquid nitrile rubber, phenolic resin, terpene resin, paraffin, and engine oil, preferably liquid nitrile rubber, and more preferably carboxyl-terminated liquid nitrile rubber.

[0019] The second object of the present invention is to provide a method for preparing the propeller material according to the first object of the present invention, the method comprising:

[0020] S1: Rubber and resin are melted together to obtain a first mixture;

[0021] S2: Blending graphite, a reinforcing agent and a plasticizer to obtain a second mixture;

[0022] S3: blending the first mixture, the second mixture, and the accelerator to obtain a third mixture;

[0023] S4: blending the third mixture with a vulcanizing agent to obtain a rubber compound;

[0024] S5: the rubber mixture is dissolved in a solvent to obtain a rubber slurry; the fiber is immersed in the rubber slurry and dried to obtain a dipped fiber;

[0025] S6: The mixed rubber is mixed with the dipped fiber to obtain a propeller preparation material.

[0026] The method for preparing the propeller material of the present invention can specifically adopt the following steps:

[0027] S1: mixing rubber and resin uniformly in a rubber mixing device, wherein the temperature in the rubber mixing device needs to meet the requirement of melting the two, to obtain a first mixture.

[0028] S2: Blending graphite, a reinforcing agent and a plasticizer, and mixing them evenly to obtain a second mixture.

[0029] S3: The first mixture and the second mixture are mixed in an internal mixer, and then an accelerator is added thereto, and the mixture is mixed evenly to obtain a third mixture.

[0030] S4: adding a vulcanizing agent to the third mixture and blending to obtain a rubber compound, wherein the temperature in the internal mixer needs to meet the vulcanization requirements.

[0031] S5: Adding a solvent to the rubber mix obtained in step S4 to prepare a rubber slurry. The amount of the solvent added is for the purpose of dissolving the rubber mix. Since the solubility of the rubber mix in different solvents is different, the amount of the solvent is not limited here. Preferably, the solvent is at least one of ethyl acetate, benzene, solvent gasoline, and xylene; more preferably, ethyl acetate. The fiber is placed in the rubber slurry, soaked for a certain period of time, and then dried to obtain a dipped fiber.

[0032] S6: mixing the dipped fiber obtained in step S5 with the rubber mixture obtained in step S4 to obtain a propeller preparation material, which can be used to prepare a propeller.

[0033] In a preferred embodiment of the present invention, in step S1, the eutectic melting temperature is 150-170° C., and the eutectic melting time is 5-15 min; and / or, in step S3, the blending temperature is 120-150° C., and the blending time is 3-8 min; and / or, in step S4, the blending temperature is 120-150° C., and the blending time is 1-5 min; and / or, in step S5, the soaking time is 16-48 h, and the drying temperature is 100-125° C. The technician can select the appropriate eutectic melting temperature, eutectic melting time, blending temperature, blending time, soaking time and drying temperature according to actual needs.

[0034] The second object of the present invention is to provide another method for preparing the propeller material according to the first object of the present invention, the preparation method comprising:

[0035] (1) blending rubber and resin to obtain a rubber compound;

[0036] (2) adding an accelerator and a plasticizer to the rubber mixture, blending the mixture, and obtaining an intermediate product;

[0037] (3) Blending graphite, reinforcing agent and fiber to obtain filler;

[0038] (4) Adding the filler into the intermediate product in multiple times, and then adding an accelerator and a vulcanizing agent to obtain a propeller preparation material.

[0039] Preferably, the filler is added to the intermediate product in 3 to 5 times.

[0040] The method for preparing the propeller material of the present invention can specifically adopt the following steps:

[0041] (1) placing rubber and resin in an internal mixer and blending them at a certain temperature to obtain a rubber mixture;

[0042] (2) Adding an accelerator and a plasticizer to the rubber mixture and blending them at a certain temperature to obtain an intermediate product.

[0043] (3) Put the graphite, reinforcing agent and fiber in a mechanical mixing device and blend them at room temperature to obtain a filler. The "mechanical mixing device" here can be an internal mixer or an open mixer.

[0044] (4) The filler prepared in step (3) is added to the intermediate product prepared in step (2) in several batches, and then an accelerator and a vulcanizing agent are added thereto to react, and finally a propeller preparation material is prepared.

[0045] It should be noted that a promoter is used in both step (2) and step (4). The promoters in the two steps may be the same or different, and the technicians may select the promoter according to the actual situation.

[0046] In a preferred embodiment of the present invention, in step (1), the blending temperature is 90-110° C., and the blending time is 5-15 min; and / or, in step (2), the blending temperature is 120-140° C., and the blending time is 2-5 min; and / or, in step (4), the reaction temperature is 120-140° C., and the reaction time is 5-10 min. The technician can select the appropriate blending temperature, blending time, reaction temperature and reaction time according to actual needs.

[0047] The third object of the present invention is to provide a propeller, which is processed and formed from the propeller preparation material described in the first object of the present invention or the propeller preparation material prepared by the preparation method described in the second object of the present invention.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] 1. The propeller preparation material of the present invention is obtained by preparing a blend using graphite, resin, rubber, and fiber materials. The propeller prepared from the propeller preparation material is light in weight, low in energy consumption, and also has excellent self-lubrication, low noise, rigidity, and recyclability (scrapped or used vulcanized rubber products can be desulfurized through a regeneration process and prepared into recycled rubber for continued use); its self-lubrication enables the propeller to have better conveying capacity for fine materials, its elasticity solves the problem of high noise in shaftless screw conveyors in the prior art, and its rigidity meets the screw pushing performance. At the same time, the propeller prepared from the propeller preparation material of the present invention also has excellent chemical corrosion resistance and acid and alkali resistance, which can extend the service life of the propeller product and solve the weakness of traditional propellers that have a short life due to acid and alkali corrosion resistance.

[0050] 2. The propeller made from the prepared material for the propeller of the present invention has a good ability to transport fine materials, and is particularly suitable for solid-liquid transport blades in manure pits, biogas, and sewage treatment systems.

[0051] 3. The method for preparing the propeller material of the present invention is simple, novel, safe and reliable, and suitable for industrial production and application. DETAILED DESCRIPTION

[0052] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0053] The raw materials used in the examples and comparative examples are all conventional commercially available raw materials.

[0054] In the present invention, the accelerator CZ is N-cyclohexyl-2-benzothiazole sulfenamide, the accelerator TDTM is tetramethylthiuram disulfide, and the accelerator TRA is dipentylenethiuram tetrasulfide.

[0055] Example 1

[0056] S1: Weigh rubber, resin, graphite, fiber, vulcanizer, accelerator, reinforcing agent, and plasticizer according to the following weight parts:

[0057]

[0058]

[0059] Among them, two substances are selected as accelerators, namely accelerator CZ and accelerator TDTM. In this embodiment, 1.5 parts by weight of accelerator CZ and 0.5 parts by weight of accelerator TDTM are weighed respectively; the molecular weight of ultra-high molecular weight polyethylene resin is 3 million molecular weight; the raw rubber Mooney viscosity of carboxylated nitrile rubber is 70, and the acrylonitrile content in carboxylated nitrile rubber is 35%; the carbon content of nano-cryptocrystalline graphite is 87%. The above rubber, resin, graphite, fiber, vulcanizer, accelerator, reinforcing agent, and plasticizer total 202 parts by weight.

[0060] S2: Mix carboxylated nitrile rubber, nitrile rubber and ultra-high molecular weight polyethylene resin evenly in a rubber mixing device, wherein the temperature in the rubber mixing device is 160° C. and the mixing time is 15 minutes to obtain a first mixture.

[0061] S3: Blending the nano-cryptocrystalline graphite, N330 carbon black and liquid nitrile rubber, and mixing them evenly to obtain a second mixture.

[0062] S4: Mix the first mixture and the second mixture in an internal mixer, add an accelerator thereto, and mix them evenly to obtain a third mixture, wherein the blending temperature is 135° C. and the blending time is 5 min.

[0063] S5: adding sulfur to the third mixture and blending to obtain a rubber compound, wherein the blending temperature is 135° C. and the blending time is 5 min.

[0064] S6: Take 20 parts by weight of the rubber mix obtained in step S5, add ethyl acetate thereto, and mix the rubber mix with 80 parts by weight of ethyl acetate to prepare a rubber slurry. Place the glass fiber in the rubber slurry, soak for 24 hours, and dry at 105° C. to obtain dipped fiber.

[0065] S7: mixing the dipped fiber obtained in step S6 with the remaining mixed rubber in step S5 to obtain a propeller preparation material, which can be used to prepare a propeller.

[0066] Example 2

[0067] S1: Weigh rubber, resin, graphite, fiber, vulcanizer, accelerator, reinforcing agent, and plasticizer according to the following weight parts:

[0068]

[0069]

[0070] The carbon content of the nano cryptocrystalline graphite is 87%. The rubber, resin, graphite, fiber, vulcanizer, accelerator, reinforcing agent and plasticizer mentioned above account for 255.5 parts by weight in total.

[0071] S2: The chlorinated polyethylene rubber and the chlorinated polyethylene resin were melt-blended in an internal mixer at 90° C. for 15 min to prepare a blend of rubber and resin.

[0072] S3: The rubber and resin blend prepared in S2, magnesium oxide, and phenolic resin are placed in an internal mixer and blended at 120° C. to obtain an intermediate product. The blending time is 5 minutes.

[0073] S4: Place nano-cryptocrystalline graphite, diatomaceous earth, N234 carbon black, N330 carbon black and aramid fiber in a mechanical mixing device and blend them at room temperature to obtain a filler, wherein the blending time is 8 minutes.

[0074] S5: Add the filler obtained in step S4 to the intermediate product obtained in step S3 in three times, add accelerator TRA and bi-25 thereto, mix well, and finally prepare the propeller preparation material. The blending temperature is 130° C. and the blending time is 5 min.

[0075] Comparative Example 1

[0076] The blades are made of "#45 high-quality carbon structural steel" using conventional blade preparation equipment in the art, wherein the #45 high-quality carbon structural steel complies with the national standard GB / T 699-2015.

[0077] The propeller prepared materials obtained in Examples 1 to 2 are used for the preparation of blades. The specific preparation method is: the prepared materials are made into blades using conventional blade preparation equipment in the art. After the blades are prepared, the steel blades of Examples 1 to 2 and Comparative Example 1 are subjected to performance tests, and the performance tests specifically include hardness test, tensile fracture strength test, self-lubricity test, wear resistance test, and corrosion resistance test. Among them, the tensile fracture strength test, self-lubricity test, wear resistance test, and corrosion resistance test are tested with reference to the test methods of GB / T528, HG / T2729, GB / T 1689 (1min grinding wheel), and GB / T 1690, respectively. The test results are shown in Table 1; the hardness test of Examples 1 to 2 refers to GB / T531.1; the hardness test of Comparative Example 1 refers to GB / T 230.1-2018.

[0078] Table 1 Performance test results of propeller blades made of prepared materials for propellers in Examples 1 to 2 and Comparative Example 1

[0079]

Claims

1. A propeller preparation material, characterized in that: The propeller material is prepared by mixing and vulcanizing raw materials including the following components: rubber, resin, graphite, fiber, vulcanizing agent, accelerator, reinforcing agent and plasticizer; The rubber is calculated by weight as 100 parts:

2. The propeller preparation material according to claim 1, characterized in that: The rubber is calculated by weight as 100 parts:

3. The propeller preparation material according to claim 1, characterized in that: The rubber is at least one of chlorinated polyethylene rubber, nitrile rubber, ethylene propylene rubber and styrene butadiene rubber, preferably carboxylated nitrile rubber; and / or The resin is at least one of polyurethane resin, polyethylene resin, chlorinated polyethylene resin, ultra-high molecular weight polyethylene resin, polypropylene resin, polystyrene resin, polyether ketone resin, polyimide resin and polyester resin, preferably ultra-high molecular weight polyethylene resin; and / or The number of layers of the graphene is less than 10, and the graphite is nanographite; and / or The fiber is a short fiber or a mesh fiber, preferably at least one of carbon fiber, aramid fiber, polyester fiber, polyimide fiber, glass fiber, basalt fiber, and synthetic fiber, more preferably a short fiber blended with polyester fiber and aramid fiber; and / or The vulcanizing agent is at least one of a peroxide vulcanizing agent, an amine vulcanizing agent, a resin vulcanizing agent, and sulfur, preferably at least one of dicumyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, hexamethylenediamine carbamate, triethylenetetramine, and sulfur; and / or The accelerator is at least one of zinc oxide, magnesium oxide, thiurams, amines, and thiazoles, preferably at least one of N-cyclohexyl-2-benzothiazole sulfenamide and phenolic resin; and / or The reinforcing agent is at least one of carbon black, white carbon black, carbon black and diatomaceous earth, preferably carbon black; and / or The plasticizer is at least one of liquid nitrile rubber, phenolic resin, terpene resin, paraffin, and engine oil, preferably liquid nitrile rubber, and more preferably carboxyl-terminated liquid nitrile rubber.

4. The propeller preparation material according to claim 3, characterized in that: The raw Mooney viscosity of the carboxylated nitrile rubber is 60 to 85; and / or The acrylonitrile content in the carboxylated nitrile rubber is 18 to 45 wt %; and / or The molecular weight of the polyethylene resin is 1.2 to 4 million; and / or The carbon content of the graphite is above 85%.

5. A method for preparing a propeller material as claimed in any one of claims 1 to 4, characterized in that The preparation method comprises: S1: Rubber and resin are melted together to obtain a first mixture; S2: Blending graphite, a reinforcing agent and a plasticizer to obtain a second mixture; S3: blending the first mixture, the second mixture, and the accelerator to obtain a third mixture; S4: blending the third mixture with a vulcanizing agent to obtain a rubber compound; S5: the rubber mixture is dissolved in a solvent to obtain a rubber slurry; the fiber is immersed in the rubber slurry and dried to obtain a dipped fiber; S6: The mixed rubber is mixed with the dipped fiber to obtain a propeller preparation material.

6. The preparation method according to claim 5, characterized in that: In step S1, the eutectic melting temperature is 150-170° C., and the eutectic melting time is 5-15 min; and / or In step S3, the blending temperature is 120-150° C., and the blending time is 3-8 min; and / or In step S4, the blending temperature is 120-150° C., and the blending time is 1-5 min; and / or In step S5, the soaking time is 16 to 48 hours, and the drying temperature is 100 to 125°C.

7. The preparation method according to claim 5, characterized in that: In step S5, the solvent is at least one of ethyl acetate, benzene, solvent gasoline, and xylene; preferably ethyl acetate.

8. A method for preparing the propeller material as claimed in any one of claims 1 to 4, characterized in that The preparation method comprises: (1) blending rubber and resin to obtain a rubber compound; (2) adding an accelerator and a plasticizer to the rubber mixture, blending the mixture, and obtaining an intermediate product; (3) Blending graphite, reinforcing agent and fiber to obtain filler; (4) adding the filler into the intermediate product in multiple times, and then adding an accelerator and a vulcanizing agent to obtain a propeller preparation material; Preferably, the filler is added to the intermediate product in 3 to 5 times.

9. The preparation method according to claim 8, characterized in that: In step (1), the blending temperature is 90 to 110° C. and the blending time is 5 to 15 min; and / or In step (2), the blending temperature is 120-140° C. and the blending time is 2-5 min; and / or In step (4), the reaction temperature is 120-140° C. and the reaction time is 5-10 min.

10. A propeller, characterized in that: The propeller preparation material is processed and formed by the propeller preparation material described in any one of claims 1 to 4 or the propeller preparation method described in any one of claims 5 to 9.