Short fiber modified and reinforced high-performance rubber and rubber V belt prepared from same
By using short fiber and nano-chitin modified rubber in the rubber V-belt, the problem of easy peeling of the skeleton material is solved, the mechanical strength and service life of the rubber V-belt are improved, and the competitiveness of the product is enhanced.
Patent Information
- Application Number
- CN202411090657.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-15
AI Technical Summary
The skeleton material of existing rubber V-belts is easy to peel off during use, resulting in a short service life and difficulty in resisting vicious low-price competition.
High-performance rubber modified and reinforced by short fibers is used. Short fibers and nano-chitin are evenly dispersed in the latex through emulsion polymerization to improve the mechanical strength of the rubber. Rubber V-belts are prepared through specific formulas and process steps to increase the skeleton line. The bonding strength of rope and rubber.
It significantly improves the mechanical strength of the rubber V-belt and the bonding strength of the skeleton cord, prolongs the service life and enhances the market competitiveness of the product.
Abstract
Description
Technical Field
[0001] The invention relates to a composite rubber material and application thereof, in particular to a short fiber modified and reinforced high-performance rubber and a rubber V-belt made therefrom. Background Art
[0002] Rubber V-belts are also called triangle belts. When working, the side of the belt is pressed against the pulley groove to generate friction for power transmission. Rubber V-belt transmission has the following advantages: 1) V-belts are elastic, running smoothly and with low noise; 2) V-belts will slip when overloaded, playing a protective role; 3) low manufacturing and installation precision requirements; 4) suitable for long-distance transmission. Therefore, rubber V-belts have been widely used in mechanical transmission.
[0003] The rubber V-belt is composed of a belt body and a rubber canvas wrapped around the belt body, wherein the belt body is composed of a top rubber, a wire core and a bottom rubber. For a rubber V-belt, the strength of the rubber itself and the bonding strength between the rubber and the skeleton wire are the key factors that determine its service life. Therefore, it is necessary to develop new rubber V-belt products with high rubber material strength and skeleton wires that are not easy to peel off, so as to improve the market competitiveness of products and resist low-price vicious competition. Summary of the invention
[0004] In order to overcome the above problems existing in the prior art, the present application provides a short fiber modified and reinforced high-performance rubber and a rubber V-belt made therefrom. The high-performance rubber of the present application is made using a specific formula process, the vulcanized rubber has high mechanical strength, and the rubber V-belt made therefrom is not prone to skeleton material peeling and has a long service life.
[0005] For rubber materials, this application provides the following technical solutions:
[0006] The high-performance rubber modified and reinforced with short fibers has the following formula proportions by weight: 100 parts of styrene-butadiene rubber, 3-6 parts of sulfur, 1-5 parts of cross-linking agent TAIC, 10-15 parts of zinc oxide, 20-30 parts of carbon black, 2-4 parts of antioxidant, 2-4 parts of coupling agent, 1-2 parts of accelerator CBS, 1-1.5 parts of accelerator TMTD, 1-1.5 parts of accelerator DTDM, 2-4 parts of stearic acid, and 1-2 parts of pine tar;
[0007] The styrene butadiene rubber is an emulsion polymerized styrene butadiene rubber, which is prepared according to the following method steps:
[0008] 1) Take SBR stripping latex, then add dispersant, nano-chitin, short fibers, stir evenly to obtain material A, and set aside;
[0009] 2) Add the coagulant and sulfuric acid solution into hot water, then add material A, coagulate under stirring to obtain colloid particles, dry and set aside;
[0010] Wherein, based on dry rubber, the amount of dispersant in step 1) is 0.1-0.5% of styrene-butadiene rubber, the amount of nano-chitin is 1-4% of styrene-butadiene rubber, and the amount of short fiber is 5-10% of styrene-butadiene rubber.
[0011] Furthermore, in the aforementioned short fiber modified and reinforced high-performance rubber, the carbon black is preferably one or more of carbon black N22045, carbon black N330, and carbon black N-220.
[0012] Furthermore, in the aforementioned short fiber modified and reinforced high-performance rubber, the antioxidant is preferably one or more of antioxidant BW-60, antioxidant BLE, and antioxidant 4010NA.
[0013] Furthermore, in the short fiber modified and reinforced high-performance rubber, the dispersant is preferably a wax dispersant. Furthermore, the dispersant is preferably microcrystalline wax.
[0014] Furthermore, in the aforementioned short fiber modified and reinforced high-performance rubber, the preparation method of the short fiber modified and reinforced high-performance rubber comprises the following steps:
[0015] (1) mixing styrene-butadiene rubber, a cross-linking agent TAIC, an antioxidant, a coupling agent, stearic acid, and pine tar, and plasticizing on an open mill, controlling the roller distance to 2-4 mm, the roller temperature to 45-55° C., and plasticizing for 10-15 minutes to obtain a plasticized rubber;
[0016] (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 1-2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 3-4 minutes, controlling the discharge temperature at 130-140° C., and producing sheets with a thickness of 8-10 mm. After cooling, a section of mixed rubber is obtained, which is left for more than 5 hours;
[0017] (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 3-4 minutes. The discharge temperature is controlled at 120-125° C. and sheets are produced with a thickness of 5-10 mm. After cooling, the second-stage rubber mix is obtained.
[0018] For rubber V-belts, this application provides the following technical solutions:
[0019] The short fiber modified and reinforced rubber V-belt comprises a belt body composed of a base rubber, a wire core skeleton and a top rubber, and a rubber canvas layer wrapped around the belt body; the rubber V-belt is made of the short fiber modified and reinforced high-performance rubber of the present application.
[0020] Further, in the aforementioned short fiber modified and reinforced rubber V-belt solution, the rubber V-belt is prepared according to the following steps:
[0021] (1) Using short fiber modified and reinforced high-performance rubber, an adhesive is produced by extrusion molding process;
[0022] (2) Using short fiber modified and reinforced high-performance rubber, a base rubber and a top rubber are produced by extrusion molding; then, the skeleton cord is wound around the top rubber;
[0023] (3) taking the short fiber modified and reinforced high-performance rubber, and calendering the short fiber modified and reinforced high-performance rubber onto the surface of the canvas by using a calender to obtain the wiped canvas;
[0024] (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank;
[0025] (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization (after vulcanization, the skeleton cord and the adhesive form the wire core skeleton of the V-belt).
[0026] Furthermore, in the aforementioned short fiber modified and reinforced rubber V-belt solution, the vulcanization temperature is 130-145° C., and the vulcanization time is 30-40 min.
[0027] Compared with the prior art, the above technical solution of the present application has achieved the following significant progress:
[0028] 1) The styrene-butadiene rubber is prepared by an emulsion polymerization method, short fibers are added to the emulsion so that the short fibers are uniformly dispersed in the rubber, and nano-chitin is added to the emulsion. The nano-chitin is combined with the short fibers to make the short fibers cationic, which effectively avoids agglomeration during the rubber refining process. The short fibers are blended and dissolved with the rubber to reinforce the rubber, so that the vulcanized rubber of the high-performance rubber of the present application has strong mechanical strength;
[0029] 2) The rubber V-belt of the present application is made of the high-performance rubber of the present application. Nano-chitin can increase the specific surface area of the skeleton cord, so that the bonding strength between the skeleton cord and the rubber is higher and not easy to peel off, thereby increasing the service life of the rubber V-belt. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with specific implementation methods (embodiments), but is not intended to be limiting of the present invention. The contents not described in detail in the following embodiments are all common technical knowledge in the art.
[0031] In the following embodiments, the short fibers used are PVC short fibers, the skeleton cords are aramid cords, and the styrene-butadiene rubber used is labeled 1502. When implementing the technical solution of the present invention, other types or models of short fibers, skeleton cords, and rubber materials may also be used without violating the principles of the present invention.
[0032] Embodiment 1:
[0033] The high-performance rubber modified and reinforced with short fibers has the following formula proportions by weight: 100 parts of styrene-butadiene rubber, 3 parts of sulfur, 5 parts of cross-linking agent TAIC, 15 parts of zinc oxide, 20 parts of carbon black, 4 parts of antioxidant, 4 parts of coupling agent, 1 part of accelerator CBS, 1 part of accelerator TMTD, 1 part of accelerator DTDM, 4 parts of stearic acid, and 1 part of pine tar;
[0034] The styrene butadiene rubber is an emulsion polymerized styrene butadiene rubber, which is prepared according to the following method steps:
[0035] 1) Take SBR stripping latex, then add dispersant, nano-chitin, short fibers, stir evenly to obtain material A, and set aside;
[0036] 2) Add the coagulant and sulfuric acid solution into hot water, then add material A, coagulate under stirring to obtain colloid particles, dry and set aside;
[0037] Wherein, based on dry rubber, the amount of dispersant in step 1) is 0.1% of styrene-butadiene rubber, the amount of nano-chitin is 1% of styrene-butadiene rubber, and the amount of short fiber is 5% of styrene-butadiene rubber.
[0038] In this embodiment, the carbon black is carbon black N22045.
[0039] In this embodiment, the antioxidant is antioxidant BW-60.
[0040] In this embodiment, the dispersant is a wax dispersant. Specifically, the dispersant is microcrystalline wax.
[0041] In this embodiment, the method for preparing the short fiber modified and reinforced high-performance rubber comprises the following steps:
[0042] (1) Styrene-butadiene rubber, cross-linking agent TAIC, antioxidant, coupling agent, stearic acid and pine tar are mixed, and plasticized on an open mill, with the roller distance controlled at 3 mm and the roller temperature controlled at 45° C., and plasticized for 15 minutes to obtain a plasticized rubber;
[0043] (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 3 minutes, controlling the discharge temperature at 130° C., and discharging the sheet with a thickness of 8 mm. After cooling, a section of mixed rubber is obtained, and the mixed rubber is left for more than 5 hours;
[0044] (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 4 minutes. The discharge temperature is controlled at 120°C and sheets are produced with a thickness of 8 mm. After cooling, the second-stage rubber mix is obtained, i.e., the high-performance rubber modified and reinforced with short fibers.
[0045] In this embodiment, the rubber V-belt includes a belt body composed of a base rubber, a wire core skeleton and a top rubber, and a rubber canvas layer wrapped around the belt body; the rubber V-belt is made of high-performance rubber modified and reinforced with short fibers in this embodiment.
[0046] In this embodiment, the rubber V-belt is prepared according to the following steps:
[0047] (1) Using short fiber modified and reinforced high-performance rubber, an adhesive is produced by extrusion molding process;
[0048] (2) Using short fiber modified and reinforced high-performance rubber, a base rubber and a top rubber are produced by extrusion molding; then, the skeleton cord is wound around the top rubber;
[0049] (3) taking the short fiber modified and reinforced high-performance rubber, and calendering the short fiber modified and reinforced high-performance rubber onto the surface of the canvas by using a calender to obtain the wiped canvas;
[0050] (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank;
[0051] (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization (the vulcanization temperature is 130° C. and the vulcanization time is 40 min).
[0052] Embodiment 2:
[0053] The high-performance rubber modified and reinforced with short fibers has the following formula proportions by weight: 100 parts of styrene-butadiene rubber, 6 parts of sulfur, 1 part of cross-linking agent TAIC, 15 parts of zinc oxide, 20 parts of carbon black, 4 parts of antioxidant, 4 parts of coupling agent, 1 part of accelerator CBS, 1.5 parts of accelerator TMTD, 1.5 parts of accelerator DTDM, 2 parts of stearic acid, and 2 parts of pine tar.
[0054] The styrene butadiene rubber is an emulsion polymerized styrene butadiene rubber, which is prepared according to the following method steps:
[0055] 1) Take SBR stripping latex, then add dispersant, nano-chitin, short fibers, stir evenly to obtain material A, and set aside;
[0056] 2) Add the coagulant and sulfuric acid solution into hot water, then add material A, coagulate under stirring to obtain colloid particles, dry and set aside;
[0057] Wherein, based on dry rubber, the amount of dispersant used in step 1) is 0.5% of the styrene-butadiene rubber, the amount of nano-chitin used is 3% of the styrene-butadiene rubber, and the amount of short fibers used is 5% of the styrene-butadiene rubber.
[0058] In this embodiment, the carbon black is carbon black N-220.
[0059] In this embodiment, the antioxidant is antioxidant BW-60.
[0060] In this embodiment, the dispersant is a wax dispersant. Specifically, the dispersant is microcrystalline wax.
[0061] In this embodiment, the method for preparing the short fiber modified and reinforced high-performance rubber comprises the following steps:
[0062] (1) Styrene-butadiene rubber, cross-linking agent TAIC, antioxidant, coupling agent, stearic acid and pine tar are mixed, and plasticized on an open mill, with the roller distance controlled at 2 mm and the roller temperature controlled at 55° C., and plasticized for 15 minutes to obtain a plasticized rubber;
[0063] (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 3 minutes, controlling the discharge temperature at 140° C., and discharging the sheet with a thickness of 10 mm. After cooling, a section of mixed rubber is obtained, which is left for more than 5 hours;
[0064] (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 4 minutes. The discharge temperature is controlled at 125°C, and sheets are produced with a thickness of 5 mm. After cooling, the second-stage rubber mix is obtained.
[0065] In this embodiment, the short fiber modified and reinforced rubber V-belt includes a belt body composed of a base rubber, a wire core skeleton and a top rubber, and a rubber canvas layer wrapped around the belt body; the rubber V-belt is made of the short fiber modified and reinforced high-performance rubber of this embodiment.
[0066] In this embodiment, the rubber V-belt is prepared according to the following steps:
[0067] (1) Using short fiber modified and reinforced high-performance rubber, an adhesive is produced by extrusion molding process;
[0068] (2) Using short fiber modified and reinforced high-performance rubber, a base rubber and a top rubber are produced by extrusion molding; then, the skeleton cord is wound around the top rubber;
[0069] (3) taking the short fiber modified and reinforced high-performance rubber, and calendering the short fiber modified and reinforced high-performance rubber onto the surface of the canvas by using a calender to obtain the wiped canvas;
[0070] (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank;
[0071] (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization (the vulcanization temperature is 145°C and the vulcanization time is 30 minutes).
[0072] Embodiment 3:
[0073] The short fiber modified and reinforced high-performance rubber is characterized in that the formula ratio is as follows by weight: 100 parts of styrene-butadiene rubber, 5 parts of sulfur, 3 parts of cross-linking agent TAIC, 12 parts of zinc oxide, 25 parts of carbon black, 3 parts of antioxidant, 3 parts of coupling agent, 1.5 parts of accelerator CBS, 1.2 parts of accelerator TMTD, 1.2 parts of accelerator DTDM, 3 parts of stearic acid, and 1.5 parts of pine tar;
[0074] The styrene butadiene rubber is an emulsion polymerized styrene butadiene rubber, which is prepared according to the following method steps:
[0075] 1) Take SBR stripping latex, then add dispersant, nano-chitin, short fibers, stir evenly to obtain material A, and set aside;
[0076] 2) Add the coagulant and sulfuric acid solution into hot water, then add material A, coagulate under stirring to obtain colloid particles, dry and set aside;
[0077] Wherein, based on dry rubber, the amount of dispersant used in step 1) is 0.3% of the styrene-butadiene rubber, the amount of nano-chitin used is 2% of the styrene-butadiene rubber, and the amount of short fibers used is 8% of the styrene-butadiene rubber.
[0078] In this embodiment, the carbon black is carbon black N-220.
[0079] In this embodiment, the antioxidant is antioxidant BLE.
[0080] In this embodiment, the dispersant is a wax dispersant. Specifically, the dispersant is microcrystalline wax.
[0081] In this embodiment, the method for preparing the short fiber modified and reinforced high-performance rubber comprises the following steps:
[0082] (1) Styrene-butadiene rubber, cross-linking agent TAIC, antioxidant, coupling agent, stearic acid and pine tar are mixed, and plasticized on an open mill, with the roller distance controlled at 3 mm and the roller temperature controlled at 50° C., and plasticized for 12 minutes to obtain a plasticized rubber;
[0083] (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 4 minutes, controlling the discharge temperature at 135° C., and discharging the sheet with a thickness of 10 mm. After cooling, a section of mixed rubber is obtained, which is left for more than 5 hours;
[0084] (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 3 minutes. The discharge temperature is controlled at 125°C, and sheets are produced with a thickness of 8 mm. After cooling, the second-stage rubber mix is obtained.
[0085] In this embodiment, the short fiber modified and reinforced rubber V-belt comprises a belt body composed of a base rubber, a wire core skeleton and a top rubber, and a rubber canvas layer wrapped around the belt body; the rubber V-belt is made of the short fiber modified and reinforced high-performance rubber of this embodiment. The rubber V-belt is made according to the following steps:
[0086] (1) Using short fiber modified and reinforced high-performance rubber, an adhesive is produced by extrusion molding process;
[0087] (2) Using short fiber modified and reinforced high-performance rubber, a base rubber and a top rubber are produced by extrusion molding; then, the skeleton cord is wound around the top rubber;
[0088] (3) taking the short fiber modified and reinforced high-performance rubber, and calendering the short fiber modified and reinforced high-performance rubber onto the surface of the canvas by using a calender to obtain the wiped canvas;
[0089] (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank;
[0090] (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization (the vulcanization temperature is 140° C. and the vulcanization time is 305 min).
[0091] Comparative Example 1 (using commercially available styrene-butadiene rubber):
[0092] In Comparative Example 1, the rubber formula ratio is as follows by weight: 100 parts of styrene-butadiene rubber, 3 parts of sulfur, 1 part of cross-linking agent TAIC, 15 parts of zinc oxide, 25 parts of carbon black, 3 parts of antioxidant, 2 parts of coupling agent, 2 parts of accelerator CBS, 1.5 parts of accelerator TMTD, 1.5 parts of accelerator DTDM, 2 parts of stearic acid, and 2 parts of pine tar.
[0093] In Comparative Example 1, the carbon black is carbon black N22045.
[0094] In Comparative Example 1, the antioxidant is antioxidant BW-60.
[0095] In Comparative Example 1, the dispersant is a wax dispersant. Specifically, the dispersant is microcrystalline wax.
[0096] In Comparative Example 1, the preparation method of rubber (rubber compound) comprises the following steps:
[0097] (1) mixing styrene-butadiene rubber, a cross-linking agent TAIC, an antioxidant, a coupling agent, stearic acid, and pine tar, and plasticizing on an open mill, controlling the roller distance to 2-4 mm, the roller temperature to 45-55° C., and plasticizing for 10-15 minutes to obtain a plasticized rubber;
[0098] (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 4 minutes, controlling the discharge temperature at 140° C., and producing sheets with a thickness of 10 mm. After cooling, a section of mixed rubber is obtained, which is left for more than 5 hours;
[0099] (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 4 minutes. The discharge temperature is controlled at 125°C and sheets are produced with a thickness of 8 mm. After cooling, the second-stage rubber mix is obtained and set aside.
[0100] In comparative example 1, the rubber V-belt comprises a belt body composed of a base rubber, a wire core skeleton and a top rubber, and a rubber-rubber canvas layer wrapped around the belt body; the rubber V-belt is made of the above-mentioned rubber in this comparative example. The rubber V-belt is made according to the following steps:
[0101] (1) Take the mixed rubber of this comparative example and use the extrusion molding process to make a bonding adhesive;
[0102] (2) Take the mixed rubber of this comparative example, and use the extrusion molding process to make a base rubber and a top rubber; then, wind the skeleton wire rope on the top rubber;
[0103] (3) taking the mixed rubber of this comparative example, and extending it to the surface of canvas by a calender to obtain a rubber-wiping canvas;
[0104] (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank;
[0105] (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization (the vulcanization temperature is 130° C. and the vulcanization time is 40 min).
[0106] Comparative Example 2 (no nano-chitin added):
[0107] In Comparative Example 2, the rubber formula ratio is as follows by weight: 100 parts of styrene-butadiene rubber, 3 parts of sulfur, 5 parts of cross-linking agent TAIC, 15 parts of zinc oxide, 30 parts of carbon black, 2 parts of antioxidant, 2 parts of coupling agent, 2 parts of accelerator CBS, 1.5 parts of accelerator TMTD, 1 part of accelerator DTDM, 3 parts of stearic acid, and 1 part of pine tar.
[0108] The styrene butadiene rubber is an emulsion polymerized styrene butadiene rubber, which is prepared according to the following method steps:
[0109] 1) Take SBR stripping latex, then add dispersant and short fibers, stir evenly to obtain material A, and set aside;
[0110] 2) Add the coagulant and sulfuric acid solution into hot water, then add material A, coagulate under stirring to obtain colloid particles, dry and set aside;
[0111] Wherein, based on dry rubber, the amount of the dispersant in step 1) is 0.3% of the styrene-butadiene rubber, and the amount of the short fiber is 5% of the styrene-butadiene rubber.
[0112] In Comparative Example 2, the carbon black is carbon black N-220.
[0113] In Comparative Example 2, the antioxidant is antioxidant BLE.
[0114] In Comparative Example 2, the dispersant is a wax dispersant. Specifically, the dispersant is microcrystalline wax.
[0115] In Comparative Example 2, the preparation method of rubber (rubber compound) comprises the following steps:
[0116] (1) Styrene-butadiene rubber, cross-linking agent TAIC, antioxidant, coupling agent, stearic acid and pine tar are mixed, and plasticized on an open mill, with the roller distance controlled to 4 mm and the roller temperature controlled to 55° C., and plasticized for 10 minutes to obtain a plasticized rubber;
[0117] (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 4 minutes, controlling the discharge temperature at 140° C., and discharging the sheet with a thickness of 8 mm. After cooling, a section of mixed rubber is obtained, which is left for more than 5 hours;
[0118] (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 4 minutes. The discharge temperature is controlled at 120°C and sheets are produced with a thickness of 8 mm. After cooling, the second-stage rubber mix is obtained and set aside.
[0119] In Comparative Example 2, the rubber V-belt comprises a belt body consisting of a base rubber, a wire core skeleton and a top rubber, and a rubber-rubber canvas layer wrapped around the belt body; the rubber V-belt is made of the rubber of Comparative Example 2. The rubber V-belt is made according to the following steps:
[0120] (1) Take the rubber of comparative example 2 and make an adhesive by extrusion molding process;
[0121] (2) Take the rubber of comparative example 2 and use the extrusion molding process to make a base rubber and a top rubber; then, wind the skeleton cord around the top rubber;
[0122] (3) taking the rubber of comparative example 2, and calendering it onto the surface of canvas by using a calender to obtain a rubber-wiping canvas;
[0123] (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank;
[0124] (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization (the vulcanization temperature is 145° C. and the vulcanization time is 40 min).
[0125] In the above-mentioned Examples 1-3 of the present application, short fibers and nano-chitin were added to the latex when preparing the latex polystyrene butadiene rubber, which improved the mechanical strength of the rubber, and the bonding strength between the rubber and the V-belt skeleton cord was also improved, so that the rubber V-belt has a longer service life. In Comparative Example 1, commercially available styrene butadiene rubber was used, and the mechanical strength of the rubber and its bonding strength with the skeleton cord were not as good as those of the present invention. In Comparative Example 2, although short fibers were added, since nano-chitin was not added, the short fibers could not be well blended and dissolved with the rubber, resulting in the mechanical strength of the rubber material not being improved, and the bonding strength with the skeleton cord was not improved.
[0126] The performance test results of the products obtained in the embodiments and comparative examples are as follows:
[0127] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Shore hardness, Hs 91 89 88 73 76 Elongation at break, % 630 627 631 465 451 Tensile strength, MPa 24.1 23.7 23.5 18.1 17.2 Cord bond strength 25.2 25.9 25.3 15.1 16.9
[0128] The above general description of the invention involved in this application and the description of its specific embodiments should not be understood as limiting the technical solutions of the invention. Based on the disclosure of this application, those skilled in the art can add, reduce or combine the disclosed technical features in the above general description or / and embodiments without violating the constituent elements of the invention involved, to form other technical solutions within the protection scope of this application.
Claims
1. High-performance rubber modified and reinforced with short fibers, It is characterized in that The formula proportions are as follows by weight: 100 parts of styrene-butadiene rubber, 3-6 parts of sulfur, 1-5 parts of cross-linking agent TAIC, 10-15 parts of zinc oxide, 20-30 parts of carbon black, 2-4 parts of antioxidant, 2-4 parts of coupling agent, 1-2 parts of accelerator CBS, 1-1.5 parts of accelerator TMTD, 1-1.5 parts of accelerator DTDM, 2-4 parts of stearic acid, 1-2 parts of pine tar; The styrene butadiene rubber is an emulsion polymerized styrene butadiene rubber, which is prepared according to the following method steps: 1) Take SBR stripping latex, then add dispersant, nano-chitin, short fibers, stir evenly to obtain material A, and set aside; 2) Add the coagulant and sulfuric acid solution into hot water, then add material A, coagulate under stirring to obtain colloid particles, dry and set aside; Wherein, based on dry rubber, the amount of dispersant in step 1) is 0.1-0.5% of styrene-butadiene rubber, the amount of nano-chitin is 1-4% of styrene-butadiene rubber, and the amount of short fiber is 5-10% of styrene-butadiene rubber.
2. The short fiber modified and reinforced high-performance rubber according to claim 1, Features: The carbon black is one or more of carbon black N22045, carbon black N330, and carbon black N-220.
3. The short fiber modified and reinforced high-performance rubber according to claim 1, Features: The antioxidant is one or more of antioxidant BW-60, antioxidant BLE, and antioxidant 4010NA.
4. The short fiber modified and reinforced high-performance rubber according to claim 1, Features: The dispersant is a wax dispersant.
5. The short fiber modified and reinforced high performance rubber according to claim 4, Features: The dispersant is microcrystalline wax.
6. The short fiber modified and reinforced high performance rubber according to claims 1-5, Features: The method for preparing the short fiber modified and reinforced high-performance rubber comprises the following steps: (1) mixing styrene-butadiene rubber, a cross-linking agent TAIC, an antioxidant, a coupling agent, stearic acid, and pine tar, and plasticizing on an open mill, controlling the roller distance to 2-4 mm, the roller temperature to 45-55° C., and plasticizing for 10-15 minutes to obtain a plasticized rubber; (2) putting the plasticized rubber obtained in step (1) into an internal mixer and mixing for 1-2 minutes; then opening the top plug, adding zinc oxide and carbon black, mixing for 3-4 minutes, controlling the discharge temperature at 130-140° C., and producing sheets with a thickness of 8-10 mm. After cooling, a section of mixed rubber is obtained, which is left for more than 5 hours; (3) The first-stage rubber mix, sulfur, accelerator CBS, accelerator TMTD, and accelerator DTDM are put into an internal mixer and mixed for 3-4 minutes. The discharge temperature is controlled at 120-125° C. and sheets are produced with a thickness of 5-10 mm. After cooling, the second-stage rubber mix is obtained.
7. A short fiber modified and reinforced rubber V-belt, comprising a belt body consisting of a base rubber, a wire core skeleton and a top rubber, and a rubber canvas layer wrapped around the belt body; Features: The rubber V-belt is made of the high-performance rubber modified and reinforced by short fibers as described in any one of claims 1-6.
8. The short fiber modified and reinforced rubber V-belt according to claim 7, Features: The rubber V-belt is prepared according to the following steps: (1) Using short fiber modified and reinforced high-performance rubber, an adhesive is produced by extrusion molding process; (2) Using short fiber modified and reinforced high-performance rubber, a base rubber and a top rubber are produced by extrusion molding; then, the skeleton cord is wound around the top rubber; (3) taking the short fiber modified and reinforced high-performance rubber, and calendering the short fiber modified and reinforced high-performance rubber onto the surface of the canvas by using a calender to obtain the wiped canvas; (4) On the laminating machine, the base glue, adhesive glue and top glue prepared in the above steps are compounded, cut and then transferred to the cloth wrapping machine, and wrapped with rubber canvas to obtain the V-belt blank; (5) The V-belt blank is installed on a vulcanization mold, and a rubber V-belt product is obtained after vulcanization.
9. The short fiber modified and reinforced rubber V-belt according to claim 8, It is characterized in that The vulcanization temperature is 130-145°C and the vulcanization time is 30-40 minutes.