Flame-retardant wear-resistant rubber material and application thereof in sand suction rubber tube

The flame-retardant and wear-resistant rubber material of modified molybdenum disulfide, carbon black and silica is prepared through electrostatic assembly technology, which solves the shortcomings of wear resistance and flame retardancy of sand-absorbing rubber tubes and significantly improves the wear resistance and wear resistance of the material. Flame retardant properties extend service life and improve safety.

CN118772502APending Publication Date: 2024-10-15BENGBU HUIHUA PIPE IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410854753.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing sand suction rubber pipe has low wear resistance and lacks flame retardancy when sucking flammable materials, which affects its service life and safety.

Method used

Use electrostatic assembly technology to prepare flame-retardant and wear-resistant rubber materials that combine modified molybdenum disulfide with carbon black and white carbon black. The wear resistance is improved through the covalent bonding and layered structure of modified molybdenum disulfide and the main rubber material. , and improve the flame retardancy through the combination of molybdenum disulfide and graphene oxide.

Benefits of technology

Significantly improves the wear resistance and flame retardant properties of rubber materials, prolongs the service life of sand suction hoses and improves use safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917795790000061
    Figure BDA0004917795790000061
  • Figure BDA0004917795790000071
    Figure BDA0004917795790000071
Patent Text Reader

Abstract

The invention discloses a flame-retardant wear-resistant rubber material which comprises the following raw materials in parts by weight: 100 parts of a rubber main material, 40-50 parts of filler and 2-3 parts of a vulcanizing agent, wherein the filler comprises carbon black, white carbon black and modified molybdenum disulfide. The invention also discloses a preparation method of the flame-retardant and wear-resistant rubber material, which comprises the following steps: mixing and vulcanizing the raw materials to obtain the flame-retardant and wear-resistant rubber material. The invention also discloses an application of the flame-retardant wear-resistant rubber material in a sand suction rubber tube. The modified molybdenum disulfide with a specific structure is matched with the carbon black and the white carbon black in a proper proportion, and a proper rubber main material is matched, so that the wear resistance, the mechanical property and the flame retardance of the rubber material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber materials, in particular to a flame retardant and wear-resistant rubber material and application thereof in a sand suction hose. Background Art

[0002] Sand suction hoses are often used to suck solid substances or granular materials such as ore sand, coal dust, cement, concrete, etc. It can be a metal tube, a rubber tube, etc. Although the metal tube has good wear resistance, it has the problem of being unable to bend and being heavy, which makes it very inconvenient to use, transport, and store. Rubber tubes have the advantages of being light and bendable, and have gradually replaced metal tubes. However, the existing sand suction rubber tubes have low wear resistance, resulting in a short service life. In addition, when sucking flammable materials such as coal dust, the flame retardancy of the sand suction rubber tube needs to be improved to improve its safety in use. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a flame retardant and wear-resistant rubber material and application thereof in a sand suction hose; the present invention has good wear resistance and flame retardancy.

[0004] The invention provides a flame retardant and wear-resistant rubber material, the raw materials of which include, by weight, 100 parts of a rubber main material, 40-50 parts of a filler, and 2-3 parts of a vulcanizing agent; wherein the filler includes carbon black, white carbon black, and modified molybdenum disulfide.

[0005] Preferably, the weight ratio of carbon black, white carbon black and modified molybdenum disulfide is 2-3:1:1.

[0006] Preferably, in the preparation process of modified molybdenum disulfide, the hexadecyltrimethylammonium bromide modified molybdenum disulfide is mixed with a graphene oxide dispersion, electrostatically assembled, and solid-liquid separated to obtain an intermediate substance; the intermediate substance is mixed with an ammonium phytate solution, electrostatically assembled, and solid-liquid separated to obtain modified molybdenum disulfide.

[0007] The invention utilizes electrostatic action to electrostatically assemble positively charged hexadecyltrimethylammonium bromide-modified molybdenum disulfide with negatively charged graphene oxide, and then electrostatically assemble with positively charged ammonium phytate to obtain modified molybdenum disulfide with a specific structure.

[0008] On the one hand, the ammonium phytate layer on the surface of the modified molybdenum disulfide contains active amino groups that can bond with carboxyl nitrile rubber through covalent bonds, so that the modified molybdenum disulfide is tightly combined with the rubber main material, and the layered structure assembled by molybdenum disulfide and graphene oxide can achieve sliding friction, thereby greatly improving the wear resistance and mechanical properties of the rubber main material, and coordinating with carbon black and white carbon black in appropriate proportions can further improve the wear resistance and mechanical properties of the rubber.

[0009] On the other hand, the ammonium phytate layer on the surface of the modified molybdenum disulfide can cooperate with the phenolic resin in the main rubber material to form a covering foaming expansion, preventing the exchange and convection of heat and oxygen, and improving the flame retardancy; and the molybdenum disulfide and graphene oxide cooperate with each other to have good physical barrier properties, which can further improve the effect of expansion flame retardancy, and the molybdenum disulfide, graphite oxide and phytic acid cooperate with each other to catalyze and promote the formation of carbon layer and dilute oxygen, thereby greatly improving its flame retardancy and avoiding the generation of fly ash. In addition, this structure can also improve the smoke suppression effect. In addition, the selection of modified molybdenum disulfide and carbon black and white carbon black in appropriate proportions can further improve its flame retardancy and smoke suppression performance.

[0010] Preferably, in the process of preparing modified molybdenum disulfide, ammonium phytate is prepared from phytic acid and melamine.

[0011] Preferably, the molar ratio of phytic acid to melamine is 1:3-4.

[0012] Preferably, melamine and phytic acid are reacted in an aqueous solution at 70-80° C. for 30-60 min to obtain ammonium phytate.

[0013] Preferably, in the preparation process of modified molybdenum disulfide, the weight ratio of hexadecyltrimethylammonium bromide modified molybdenum disulfide to graphene oxide is 1:1.1-1.3.

[0014] The above-mentioned hexadecyltrimethylammonium bromide-modified molybdenum disulfide can be purchased from the market.

[0015] Preferably, in the preparation process of modified molybdenum disulfide, the weight ratio of the intermediate substance to ammonium phytate is 1:1.5-2.

[0016] Preferably, the pH of the ammonium phytate solution is 5-6.

[0017] Preferably, during the preparation of the modified molybdenum disulfide, the electrostatic assembly is performed at room temperature for 30-60 minutes.

[0018] Preferably, in the preparation process of modified molybdenum disulfide, the main rubber ingredients include: carboxylated nitrile rubber and phenolic resin.

[0019] Preferably, the weight ratio of carboxylated nitrile rubber to phenolic resin is 8-9:1-2.

[0020] The present invention selects carboxyl nitrile rubber and phenolic resin to be matched with each other in a suitable ratio, which can further improve the wear resistance and mechanical properties.

[0021] Preferably, the raw materials also include: a softener, a compatibilizer and zinc oxide.

[0022] Preferably, the weight ratio of the rubber main material to the softener, the compatibilizer and the zinc oxide is 100:1-2:3-5:4-5.

[0023] The invention adds a proper amount of softener, compatibilizer and zinc oxide, which can further promote the uniform dispersion of filler and rubber main material, thereby further improving the mechanical properties thereof, and zinc oxide can further promote the formation of a carbon layer during combustion, thereby improving the flame retardancy.

[0024] The present invention also provides a method for preparing the flame retardant and wear resistant rubber material, which comprises the following steps: mixing and vulcanizing various raw materials to obtain the flame retardant and wear resistant rubber material.

[0025] The invention also proposes the application of the flame-retardant and wear-resistant rubber material in a sand-absorbing rubber hose.

[0026] The present invention modifies molybdenum disulfide to make it have a specific structure, and combines it with carbon black and white carbon black in an appropriate proportion and a suitable rubber main material, which can improve the wear resistance and mechanical properties of the rubber material on the one hand, and improve the flame retardant properties of the rubber material on the other hand, thereby improving the service life and safety of the rubber tube. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is described in detail below through specific embodiments.

[0028] Example 1

[0029] A flame retardant and wear-resistant rubber material, the raw materials of which include, by weight: 80 parts of carboxyl nitrile rubber, 20 parts of phenolic resin, 20 parts of carbon black, 10 parts of white carbon black, 10 parts of modified molybdenum disulfide, 3 parts of sulfur, 1 part of softener stearic acid, 5 parts of compatibilizer, and 4 parts of zinc oxide;

[0030] In the preparation process of modified molybdenum disulfide, 0.1 g of hexadecyltrimethylammonium bromide-modified molybdenum disulfide is evenly dispersed in water, mixed with an aqueous dispersion containing 0.13 g of graphene oxide, stirred and mixed, electrostatically assembled at room temperature for 30 minutes, filtered, and the filter cake was washed with water to obtain an intermediate substance;

[0031] 4 mmol of melamine was evenly dispersed in water, 1 mmol of phytic acid was added and mixed, the mixture was heated to 80°C and reacted for 30 min, the mixture was filtered, the filter cake was washed with water, and the mixture was dried under reduced pressure to obtain ammonium phytate;

[0032] 0.1 g of the intermediate material and 0.2 g of ammonium phytate were uniformly dispersed in water, the pH was adjusted to 6, the mixture was stirred and evenly mixed, and electrostatic assembly was performed at room temperature for 30 min. The mixture was filtered, the filter cake was washed with water, and dried under reduced pressure to obtain modified molybdenum disulfide.

[0033] The preparation method of the flame retardant and wear-resistant rubber material comprises the following steps: mixing carboxylated nitrile rubber, phenolic resin, carbon black, white carbon black, modified molybdenum disulfide, softener stearic acid, compatibilizer and zinc oxide, kneading at 120°C, then adding sulfur and mixing, and vulcanizing at 160°C for 12 minutes to obtain a flame retardant and wear-resistant rubber material.

[0034] Example 2

[0035] A flame retardant and wear-resistant rubber material, the raw materials of which include, by weight: 90 parts of carboxyl nitrile rubber, 10 parts of phenolic resin, 30 parts of carbon black, 10 parts of white carbon black, 10 parts of modified molybdenum disulfide, 2 parts of sulfur, 2 parts of softener stearic acid, 3 parts of compatibilizer, and 5 parts of zinc oxide;

[0036] In the preparation process of modified molybdenum disulfide, 0.1 g of hexadecyltrimethylammonium bromide-modified molybdenum disulfide is evenly dispersed in water, mixed with an aqueous dispersion containing 0.11 g of graphene oxide, stirred and mixed, electrostatically assembled at room temperature for 60 minutes, filtered, and the filter cake was washed with water to obtain an intermediate substance;

[0037] 3 mmol of melamine was uniformly dispersed in water, 1 mmol of phytic acid was added and mixed, the mixture was heated to 70°C and reacted for 60 min, the mixture was filtered, the filter cake was washed with water, and the mixture was dried under reduced pressure to obtain ammonium phytate;

[0038] 0.1 g of the intermediate material and 0.15 g of ammonium phytate were uniformly dispersed in water, the pH was adjusted to 5, the mixture was stirred and evenly mixed, electrostatic assembly was performed at room temperature for 60 min, the mixture was filtered, the filter cake was washed with water, and the mixture was dried under reduced pressure to obtain modified molybdenum disulfide.

[0039] The preparation method of the flame retardant and wear-resistant rubber material comprises the following steps: mixing carboxylated nitrile rubber, phenolic resin, carbon black, white carbon black, modified molybdenum disulfide, softener stearic acid, compatibilizer and zinc oxide, kneading at 120°C, then adding sulfur and mixing, and vulcanizing at 160°C for 12 minutes to obtain a flame retardant and wear-resistant rubber material.

[0040] Example 3

[0041] A flame retardant and wear-resistant rubber material, the raw materials of which include, by weight: 85 parts of carboxyl nitrile rubber, 15 parts of phenolic resin, 25 parts of carbon black, 10 parts of white carbon black, 10 parts of modified molybdenum disulfide, 2.5 parts of sulfur, 1.5 parts of softener stearic acid, 4 parts of compatibilizer, and 4.5 parts of zinc oxide;

[0042] In the preparation process of modified molybdenum disulfide, 0.1 g of hexadecyltrimethylammonium bromide-modified molybdenum disulfide is evenly dispersed in water, mixed with an aqueous dispersion containing 0.12 g of graphene oxide, stirred and mixed, electrostatically assembled at room temperature for 40 minutes, filtered, and the filter cake was washed with water to obtain an intermediate substance;

[0043] 3.5 mmol of melamine was uniformly dispersed in water, 1 mmol of phytic acid was added and mixed, the mixture was heated to 75°C and reacted for 60 min, the mixture was filtered, the filter cake was washed with water, and the mixture was dried under reduced pressure to obtain ammonium phytate;

[0044] 0.1 g of the intermediate material and 0.17 g of ammonium phytate were uniformly dispersed in water, the pH was adjusted to 5.5, the mixture was stirred and evenly mixed, and electrostatic assembly was performed at room temperature for 40 min. The mixture was filtered, the filter cake was washed with water, and dried under reduced pressure to obtain modified molybdenum disulfide.

[0045] The preparation method of the flame retardant and wear-resistant rubber material comprises the following steps: mixing carboxylated nitrile rubber, phenolic resin, carbon black, white carbon black, modified molybdenum disulfide, softener stearic acid, compatibilizer and zinc oxide, kneading at 120°C, then adding sulfur and mixing, and vulcanizing at 160°C for 12 minutes to obtain a flame retardant and wear-resistant rubber material.

[0046] Comparative Example 1

[0047] A flame retardant and wear-resistant rubber material, wherein the modified molybdenum disulfide is hexadecyltrimethylammonium bromide modified molybdenum disulfide, and the rest is the same as in Example 3.

[0048] Comparative Example 2

[0049] A flame retardant and wear resistant rubber material, wherein modified molybdenum disulfide is the intermediate substance obtained in Example 3, and the rest is the same as Example 3.

[0050] Comparative Example 3

[0051] A flame retardant and wear-resistant rubber material, wherein the modified molybdenum disulfide is composed of hexadecyltrimethylammonium bromide-modified molybdenum disulfide and ammonium phytate in a weight ratio of 1:1.7, and the rest is the same as Example 3.

[0052] Comparative Example 4

[0053] A flame retardant and wear resistant rubber material, which does not contain modified molybdenum disulfide and is the same as Example 3 in other aspects.

[0054] Comparative Example 5

[0055] A flame retardant and wear-resistant rubber material, which does not contain phenolic resin, has 100 parts of carboxyl nitrile rubber, and the rest is the same as Example 3.

[0056] The rubber materials described in Examples 1-3 and Comparative Examples 1-5 were taken and their properties were tested respectively. The results are shown in Table 1.

[0057] UL94 and limiting oxygen index are tested according to GB-T 10707-2008.

[0058] The tensile properties were tested according to GB / T 528-2009; the abrasion resistance was tested according to ISO4649:2002 Method A.

[0059] Table 1 Test results

[0060]

[0061]

[0062] It can be seen from Table 1 that the rubber material of the present invention has good flame retardancy and wear resistance.

[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A flame retardant and wear-resistant rubber material, characterized in that: The raw materials include, by weight: 100 parts of rubber main material, 40-50 parts of filler, and 2-3 parts of vulcanizer; wherein the filler includes: carbon black, white carbon black and modified molybdenum disulfide.

2. The flame retardant and wear resistant rubber material according to claim 1, characterized in that: The weight ratio of carbon black, white carbon black and modified molybdenum disulfide is 2-3:1:

1.

3. The flame retardant and wear resistant rubber material according to claim 1 or 2, characterized in that: In the preparation process of modified molybdenum disulfide, hexadecyltrimethylammonium bromide modified molybdenum disulfide is mixed with graphene oxide dispersion, electrostatic assembly is performed, and solid-liquid separation is performed to obtain an intermediate substance; the intermediate substance is mixed with ammonium phytate solution, electrostatic assembly is performed, and solid-liquid separation is performed to obtain modified molybdenum disulfide.

4. The flame retardant and wear resistant rubber material according to claim 3, characterized in that: In the preparation process of modified molybdenum disulfide, ammonium phytate is prepared from phytic acid and melamine; preferably, the molar ratio of phytic acid to melamine is 1:3-4; preferably, melamine and phytic acid are reacted in an aqueous solution at 70-80°C for 30-60 minutes to obtain ammonium phytate.

5. The flame retardant and wear resistant rubber material according to claim 3 or 4, characterized in that: In the preparation process of modified molybdenum disulfide, the weight ratio of hexadecyltrimethylammonium bromide modified molybdenum disulfide to graphene oxide is 1:1.1-1.3; preferably, in the preparation process of modified molybdenum disulfide, the weight ratio of the intermediate substance to ammonium phytate is 1:1.5-2; preferably, the pH of the ammonium phytate solution is 5-6.

6. The flame retardant and wear resistant rubber material according to any one of claims 3 to 5, characterized in that: During the preparation of modified molybdenum disulfide, electrostatic assembly was performed at room temperature for 30-60 minutes.

7. The flame retardant and wear resistant rubber material according to any one of claims 1 to 6, characterized in that: In the preparation process of modified molybdenum disulfide, the main rubber ingredients include: carboxylated nitrile rubber and phenolic resin; preferably, the weight ratio of carboxylated nitrile rubber to phenolic resin is 8-9:1-2.

8. The flame retardant and wear resistant rubber material according to any one of claims 1 to 7, characterized in that: The raw materials also include: softener, compatibilizer, zinc oxide; preferably, the weight ratio of the rubber main material to the softener, compatibilizer, zinc oxide is 100:1-2:3-5:4-5.

9. A method for preparing the flame retardant and wear resistant rubber material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing and vulcanizing various raw materials to obtain a flame retardant and wear-resistant rubber material.

10. Use of the flame retardant and wear resistant rubber material according to any one of claims 1 to 8 in a sand suction hose.