Polypropylene resin composition as well as preparation method and application thereof

By adding a polymer nucleating agent during the propylene polymerization process, a homopolymerized polypropylene resin with excellent rigidity and heat resistance is prepared, which solves the problem of warping and deformation of the homopolymerized polypropylene resin in the existing technology under a short molding cycle. problem, achieving a polypropylene resin composition with high rigidity, high heat resistance and low shrinkage.

CN118772533APending Publication Date: 2024-10-15SHANDONG JINGBO POLYOLEFIN NEW MATERIALS CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410949827.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively improve the crystallinity and rigidity of homopolypropylene resin under a short molding cycle, resulting in warpage and deformation problems of injection molded products, and extending the molding cycle will increase production costs.

Method used

In the propylene polymerization process, a polymer nucleating agent is added to prepare a homopolymer polypropylene resin containing a polymer nucleating agent, which is mixed with an antioxidant and a halogen absorbing agent and then extruded and granulated to form a resin with excellent rigidity and durability. Thermal and dimensional stable polypropylene resin composition.

Benefits of technology

The uniformly dispersed polymer nucleating agent is realized, which improves the rigidity and heat resistance of polypropylene resin, while reducing the shrinkage rate, ensuring the high rigidity, high heat resistance and dimensional stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946893120000091
    Figure BDA0004946893120000091
  • Figure BDA0004946893120000101
    Figure BDA0004946893120000101
  • Figure BDA0004946893120000102
    Figure BDA0004946893120000102
Patent Text Reader

Abstract

The invention provides a polypropylene resin composition as well as a preparation method and application thereof. The polypropylene resin composition comprises homo-polypropylene resin containing a macromolecular nucleating agent, an antioxidant and a halogen absorbing agent. Wherein the polymer nucleating agent is added in a propylene polymerization stage instead of a common processing granulation stage in the prior art. Therefore, the polymer nucleating agent in the homo-polypropylene resin can be dispersed more uniformly, and the homo-polypropylene resin is more stable in performance. The polypropylene resin is prepared from the homo-polypropylene resin containing the macromolecular nucleating agent, so that the shrinkage rate of the polypropylene resin is reduced while high rigidity and high heat resistance of the polypropylene resin are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polypropylene resin composition and a preparation method and application thereof. Background Art

[0002] Polypropylene resin has been widely used in the fields of electronic appliances, food containers, household items, etc. due to its excellent physical and mechanical properties, heat resistance and chemical resistance. Among them, homopolymer polypropylene (PPH) resin has the advantages of high rigidity and good heat resistance. Studies have shown that improving the crystallinity of homopolymer polypropylene resin can help further improve its rigidity and heat resistance. At the same time, for the injection molding of homopolymer polypropylene, a higher crystallization rate and crystallinity can reduce the shrinkage of the material, thereby reducing the warping and deformation of the injection molded products. Therefore, it is very important to improve the crystallization performance of homopolymer polypropylene.

[0003] At present, in order to improve the crystallization performance of homopolymer polypropylene and obtain high rigidity and high heat-resistant polypropylene materials, the existing method is usually to add α nucleating agents during the material processing and granulation process to improve the crystallinity and crystallization rate of homopolymer polypropylene resin. The commonly used and effective α nucleating agents are organic small molecule nucleating agents, mainly including fatty acids and their metal soaps, dibenzylidene sorbitol and organic phosphates. However, general manufacturers improve production efficiency by shortening the product molding cycle. Under a shorter molding cycle, high rigidity and high heat-resistant PPH injection molded products have serious warping and deformation problems. The most effective way to solve the problem of warping and deformation of high rigidity and high heat-resistant PPH products is to extend the product molding cycle. However, the extension of the molding cycle will increase the product processing cost. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a polypropylene resin composition and a preparation method and application thereof. The polypropylene resin composition has excellent rigidity, heat resistance and dimensional stability.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a polypropylene resin composition comprising, by weight:

[0007] 100 parts by weight of a homopolymer polypropylene resin containing a polymer nucleating agent;

[0008] 0.1-0.3 parts by weight of antioxidant;

[0009] 0.01-0.1 parts by weight of halogen absorbent;

[0010] The homopolymer polypropylene resin containing a polymer nucleating agent is prepared by adding a polymer nucleating agent during propylene polymerization;

[0011] The mass percentage of the polymer nucleating agent in the homopolymerized polypropylene resin containing the polymer nucleating agent is 30 to 50 ppm.

[0012] Preferably, the polypropylene resin composition has a melt index of 10 to 30 g / 10 min at 230° C. / 2.16 kg, a crystallization temperature of >125° C., a heat deformation temperature of >120° C., and a transverse and longitudinal shrinkage rate of <1.2%.

[0013] Preferably, the mass percentage of isotactic polypropylene in the homopolymer polypropylene resin containing the polymer nucleating agent is 98-99.5%.

[0014] Preferably, the polymer nucleating agent is selected from any one or more of polyvinylcyclopentane, polyvinylcyclohexane, polyvinyl-2-methylcyclohexane, poly-3-methyl-1-butene, poly-3-ethyl-1-hexene, poly-3-methyl-1-pentene or polystyrene.

[0015] Preferably, the halogen absorbent is selected from any one or more of sodium stearate, calcium stearate or zinc stearate.

[0016] Preferably, the antioxidant includes a primary antioxidant and a secondary antioxidant.

[0017] Preferably, the primary antioxidant is selected from any one or more of antioxidant 2246, antioxidant 1010, antioxidant 1076 or antioxidant 1330.

[0018] Preferably, the auxiliary antioxidant is selected from any one or more of antioxidant 168, antioxidant 626 and antioxidant 9228.

[0019] Preferably, the mass ratio of the primary antioxidant to the secondary antioxidant is 1:(1-4).

[0020] In a second aspect, the present invention provides a method for preparing the above-mentioned polypropylene resin composition, comprising:

[0021] Adding a polymer nucleating agent during the propylene polymerization process to obtain a homopolymerized polypropylene resin containing the polymer nucleating agent;

[0022] A homopolymer polypropylene resin containing a polymer nucleating agent, an antioxidant and a halogen absorbent are mixed, extruded and granulated to obtain a polypropylene resin composition.

[0023] Preferably, the homopolymer polypropylene resin containing a polymer nucleating agent is prepared according to the following method:

[0024] S1: prepolymerizing a mixture of a catalyst and a polymer nucleating agent with propylene, an external electron donor, and an alkyl aluminum to obtain a propylene prepolymer;

[0025] S2: Polymerizing a propylene prepolymer and propylene in the presence of hydrogen to obtain a homopolymerized polypropylene resin containing a polymer nucleating agent.

[0026] Preferably, the catalyst is selected from Ziegler-Natta catalysts.

[0027] Preferably, the external electron donor is a silane compound, and the silane compound is selected from vinyl triethoxysilane, vinyl trimethoxysilane, methyl triethoxysilane, dimethyl dimethoxysilane, diethyl dimethoxysilane, dipropyl dimethoxysilane, diisopropyl dimethoxysilane, dibutyl dimethoxysilane, diisobutyl dimethoxysilane, di-tert-butyl dimethoxysilane, di-tert-hexyl dimethoxysilane, diphenyl dimethoxysilane, dicyclohexyl dimethoxysilane, dicyclopentyl dimethoxysilane, dimethyl diethoxysilane, diethyl diethoxysilane, dipropyl Any one or more of dimethoxysilane, diisopropyldiethoxysilane, dibutyldiethoxysilane, diisobutyldiethoxysilane, di-tert-butyldiethoxysilane, di-tert-hexyldiethoxysilane, diphenyldiethoxysilane, dicyclohexyldiethoxysilane, dicyclopentyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, cyclopentylmethyldimethoxysilane, cyclopentyltrimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexyltrimethoxysilane, tert-hexyltrimethoxysilane, tert-butyltrimethoxysilane or tert-hexyltrimethoxysilane.

[0028] Preferably, the alkylaluminum is selected from any one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum monochloride, diisobutylaluminum monochloride, dihexylaluminum monochloride or dioctylaluminum monochloride.

[0029] Preferably, the prepolymerization temperature in step S1 is -10 to 20°C and the time is 10 to 30 minutes.

[0030] Preferably, the polymerization temperature in step S2 is 50-100° C., the pressure is 1-5 MPa, and the time is 1-5 h.

[0031] In a third aspect, the present invention provides a product, which is made of the polypropylene resin composition involved in the above technical solution;

[0032] The products include automobile parts or home appliance parts.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention provides a polypropylene resin composition, which comprises: a homopolymer polypropylene resin containing a polymer nucleating agent, an antioxidant and a halogen absorbent. The polymer nucleating agent is added in the propylene polymerization stage, rather than in the usual processing and granulation stage in the prior art. In this way, the polymer nucleating agent in the homopolymer polypropylene resin can be dispersed more evenly, and the performance of the homopolymer polypropylene resin can be more stable. In addition, the polymer nucleating agent in the present invention has a low dosage, good dispersion effect, and good nucleating effect. Due to the good nucleating effect, the rigidity and heat resistance of the product are good; the nucleating agent is used in a low dosage, and the product has a low shrinkage rate and good dimensional stability. Therefore, the present invention adopts a homopolymer polypropylene resin containing a polymer nucleating agent to prepare a polypropylene resin, which not only ensures that it has high rigidity and high heat resistance, but also reduces its shrinkage rate.

[0035] The test shows that the polypropylene resin composition has excellent rigidity, heat resistance and dimensional stability, with a melt index of 10-30 g / 10 min (230° C. / 2.16 kg), a crystallization temperature of >125° C., a heat deformation temperature of >120° C., a transverse and longitudinal shrinkage rate of <1.2%, and a flexural modulus of >2000 MPa. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In view of the problems that high-rigidity and high-heat-resistant PPH injection molded products are prone to warping and deformation in a short cycle in the prior art, the present invention provides a polypropylene resin composition, which comprises, by weight:

[0038] 100 parts by weight of a homopolymer polypropylene resin containing a polymer nucleating agent;

[0039] 0.1-0.3 parts by weight of antioxidant;

[0040] 0.01~0.1 weight part of halogen absorbent.

[0041] In the present invention, the polypropylene resin composition comprises 100 weight parts of homopolymerized polypropylene resin containing polymer nucleating agent by weight. Wherein, the homopolymerized polypropylene resin containing polymer nucleating agent is prepared by adding polymer nucleating agent in the process of propylene polymerization, which is different from the usual processing and granulation stage addition in the prior art. In this way, the polymer nucleating agent in the homopolymerized polypropylene resin can be dispersed more evenly, and the homopolymerized polypropylene resin performance is more stable. Wherein, the polymer nucleating agent is selected from any one or more of polyvinylcyclopentane, polyvinylcyclohexane, polyvinyl-2-methylcyclohexane, poly-3-methyl-1-butene, poly-3-ethyl-1-hexene, poly-3-methyl-1-pentene or polystyrene, preferably polyvinylcyclohexane and / or poly-3-methyl-1-butene. In some embodiments of the present invention, the polymer nucleating agent includes polyvinyl cyclohexane and poly 3-methyl-1-butene, and the mass ratio of polyvinyl cyclohexane to poly 3-methyl-1-butene is 1:(0.8-1.5), preferably 1:(0.9-1.2), and more preferably 1:1.

[0042] In the present invention, the mass percentage of the polymer nucleating agent in the homopolymerized polypropylene resin containing the polymer nucleating agent is 30-50ppm, such as 30ppm, 32ppm, 34ppm, 36ppm, 38ppm, 40ppm, 42ppm, 44ppm, 46ppm, 48ppm or 50ppm, etc. It can be seen that in the present invention, the amount of the polymer nucleating agent is relatively low, specifically about one tenth of the normal small molecule nucleating agent (the addition amount is 500-2000ppm), but the nucleating effect is significantly better than that of the small molecule nucleating agent, therefore, the nucleating efficiency of the polymer nucleating agent used in the present invention is relatively high.

[0043] It should be noted that the point values ​​listed above in the present invention are only for enumeration and are not limited thereto. Other point values ​​within the numerical range are applicable. To avoid complexity, they will not be described one by one.

[0044] In the present invention, the mass percentage of isotactic polypropylene in the homopolymerized polypropylene resin containing a polymer nucleating agent is above 98%, specifically 98-99.5%. In the present invention, the high isotacticity of the homopolymerized polypropylene resin is beneficial to improving the rigidity and heat resistance of the product.

[0045] In the present invention, the polypropylene resin composition includes 0.1 to 0.3 parts by weight of antioxidant, preferably 0.15 to 0.2 parts, and more preferably 0.16 to 0.18 parts by weight. In the present invention, the antioxidant is used to improve the heat-oxidative aging resistance of the polypropylene resin composition, including a primary antioxidant and a secondary antioxidant. The primary antioxidant is selected from any one or more of antioxidant 2246, antioxidant 1010, antioxidant 1076 or antioxidant 1330; the secondary antioxidant is selected from any one or more of antioxidant 168, antioxidant 626 and antioxidant 9228. In some embodiments of the present invention, the mass ratio of the primary antioxidant to the secondary antioxidant is 1: (1 to 4), preferably 1: (2 to 3). In some specific embodiments of the present invention, it is preferred that antioxidant 1010 and antioxidant 168 are in a mass ratio of 1: 2, and the total content is preferably 0.15 parts by weight, as a raw material for preparing the polypropylene resin composition.

[0046] In the present invention, the polypropylene resin composition includes 0.01 to 0.1 parts by weight of a halogen absorbent, preferably 0.03 to 0.08 parts, and more preferably 0.04 to 0.06 parts by weight. In the present invention, the halogen absorbent is used to neutralize chlorine and other halogens remaining in polypropylene to prevent them from corroding equipment during processing. In the present invention, the halogen absorbent is selected from any one or more of sodium stearate, calcium stearate or zinc stearate, preferably calcium stearate. In some embodiments of the present invention, 0.06 parts of calcium stearate is preferably used.

[0047] The present invention also provides a method for preparing the above-mentioned polypropylene resin composition, which comprises:

[0048] Adding a polymer nucleating agent during the propylene polymerization process to obtain a homopolymerized polypropylene resin containing the polymer nucleating agent;

[0049] A homopolymer polypropylene resin containing a polymer nucleating agent, an antioxidant and a halogen absorbent are mixed, extruded and granulated to obtain a polypropylene resin composition.

[0050] In the present invention, a homopolymer polypropylene resin containing a polymer nucleating agent is first provided, which is prepared by adding a polymer nucleating agent during propylene polymerization. In some embodiments of the present invention, the homopolymer polypropylene resin containing a polymer nucleating agent is prepared according to the following method:

[0051] S1: prepolymerizing a mixture of a catalyst and a polymer nucleating agent with propylene, an external electron donor, and an alkyl aluminum to obtain a propylene prepolymer;

[0052] S2: Polymerizing a propylene prepolymer and propylene in the presence of hydrogen to obtain a homopolymerized polypropylene resin containing a polymer nucleating agent.

[0053] According to the present invention, firstly, a mixture of a catalyst and a polymer nucleating agent is subjected to propylene prepolymerization with propylene, an external electron donor, and an alkyl aluminum to obtain a propylene prepolymer. The catalyst is selected from a Ziegler-Natta catalyst; the external electron donor is used to adjust the isotacticity of polypropylene and is a silane compound, and the silane compound includes but is not limited to vinyl triethoxysilane, vinyl trimethoxysilane, methyl triethoxysilane, dimethyl dimethoxysilane, diethyl dimethoxysilane, dipropyl dimethoxysilane, diisopropyl dimethoxysilane, dibutyl dimethoxysilane, diisobutyl dimethoxysilane, di-tert-butyl dimethoxysilane, di-tert-hexyl dimethoxysilane, diphenyl dimethoxysilane, dicyclohexyl dimethoxysilane, dicyclopentyl dimethoxysilane, dimethyl diethoxysilane, diethyl diethoxysilane, dipropyl dieth ...isobutyl dimethoxysilane, di-tert-butyl dimethoxysilane, di-tert-hexyl dimethoxysilane, diphenyl dimethoxysilane, dicyclohexyl dimethoxysilane, dicyclopentyl dimethoxysilane, dimethyl diethoxysilane, diethyl diethoxysilane, dipropyl diethoxysilane, diisopropyl dimethoxysilane, diisobutyl dimethoxysilane, di-tert-butyl dimethoxysilane, di-tert-hexyl dimethoxysilane, di-tert-butyl dimethoxysilane, di Any one or more of silane, diisopropyldiethoxysilane, dibutyldiethoxysilane, diisobutyldiethoxysilane, di-tert-butyldiethoxysilane, di-tert-hexyldiethoxysilane, diphenyldiethoxysilane, dicyclohexyldiethoxysilane, dicyclopentyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, cyclopentylmethyldimethoxysilane, cyclopentyltrimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexyltrimethoxysilane, tert-hexyltrimethoxysilane, tert-butyltrimethoxysilane or tert-hexyltrimethoxysilane, preferably dicyclopentyldimethoxysilane; the alkylaluminum is used to reduce the active center ions of the catalyst to make the catalyst active. , specifically including but not limited to any one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum monochloride, diisobutylaluminum monochloride, dihexylaluminum monochloride or dioctylaluminum monochloride, preferably triethylaluminum.

[0054] In some embodiments of the present invention, the catalyst and the polymer nucleating agent are first mixed in a solvent at 10-30° C., filtered, and dried to obtain a mixture A of the catalyst and the polymer nucleating agent. The solvent is selected from any one or more of n-pentane, isopentane, n-hexane, or n-heptane. The mixing is preferably performed under stirring conditions.

[0055] Then, the mixture is prepolymerized with propylene, an external electron donor, and an alkyl aluminum, and the prepolymerization is preferably carried out in a prepolymerization kettle. In the present invention, propylene, an external electron donor, an alkyl aluminum, and a mixture A are preferably added sequentially into a prepolymerization kettle at -10 to 20° C. to carry out propylene prepolymerization for 10 to 30 minutes, and more preferably, prepolymerized in a polymerization kettle at 0 to 10° C. for 15 to 20 minutes to obtain a propylene prepolymer.

[0056] After obtaining the propylene prepolymer, according to the present invention, the propylene prepolymer and propylene are polymerized in the presence of hydrogen. The polymerization is preferably carried out in a polymerization kettle. In some embodiments of the present invention, the propylene prepolymer is preferably transferred from the prepolymerization kettle to the polymerization kettle, and appropriate amounts of hydrogen and propylene are added, the temperature is increased, and the propylene polymerization is carried out at a temperature of 50 to 100° C. and a pressure of 1 to 5 MPa for 1 to 5 hours, more preferably at a temperature of 70 to 80° C. and a pressure of 2 to 3 MPa for 1.5 to 3 hours, to obtain a homopolymerized polypropylene resin containing a polymer nucleating agent.

[0057] Then, according to the present invention, a homopolymerized polypropylene resin containing a polymer nucleating agent, an antioxidant and a halogen absorbent are mixed, extruded and granulated to obtain a polypropylene resin composition.

[0058] In some embodiments of the present invention, during processing, it is preferred to premix the homopolymer polypropylene resin, antioxidant and halogen absorbent in a high-speed mixer in proportion. The mixed material is fed into a twin-screw extruder by a feeder. The material is sheared and blended by the twin-screw extruder and extruded from the die. According to needs, it can be packaged after subsequent drawing, air cooling, pelletizing, drying. In the preparation method, the temperature of each section of the screw is controlled between 170 and 190°C. In some specific embodiments of the present invention, the temperature of each zone of the extruder is: 170°C in zone one, 180°C in zone two, 190°C in zone three, 190°C in zone four, 185°C in zone five, and 180°C in the die.

[0059] The test shows that the polypropylene resin composition has the characteristics of high rigidity, high heat resistance and low shrinkage, and is characterized by: crystallization temperature>125°C; bending modulus>2000MPa; heat deformation temperature>120°C; longitudinal shrinkage<1.2%; and transverse shrinkage<1.2%.

[0060] It should be noted that the crystallization temperature represents the crystallization performance of the material. The higher the crystallization temperature of the same material, the better the crystallization performance; the bending modulus represents the rigidity, and the larger the rigidity, the better; the heat deformation temperature represents the heat resistance, and the larger the better; the longitudinal shrinkage rate and the transverse shrinkage rate represent the dimensional stability, and the smaller the size, the less likely the material is to warp and deform.

[0061] Based on this, the present invention also provides an application of the homopolymerized polypropylene resin composition, such as a product, which is composed of the polypropylene resin composition involved in the above technical solution. The product can be automotive parts, such as car bodies and interior decorations, etc.; home appliance parts, such as heat-resistant parts, microwave oven containers, etc.

[0062] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention are all common commercially available products.

[0063] Example 1

[0064] Preparation of homopolymer polypropylene:

[0065] (1) 10 g of CS-1 catalyst (Liaoning Xiangyang) and 10 g of polyvinylcyclohexane (PVCH, prepared according to the method disclosed in patent application No. 202410183936.6) were stirred and blended in 1 L of n-hexane at 10° C., and then filtered and dried to obtain a catalyst and nucleating agent mixture A;

[0066] (2) At 10° C., 1 kg of propylene, 0.25 mL of dicyclopentyldimethoxysilane, 6 mL of triethylaluminum (1 M) and 0.12 g of mixture A were sequentially added into a 3 L prepolymerization reactor to carry out propylene prepolymerization for 15 min;

[0067] (3) transferring the propylene prepolymer from the prepolymerization kettle to a 10 L polymerization kettle, adding 17 L of hydrogen and 2 kg of propylene, raising the temperature, and polymerizing the propylene at 70° C. and 3 MPa for 1.5 h to obtain 2000 g of homopolypropylene;

[0068] Processing and granulation: The materials were weighed according to the components and formulas provided in Table 1 (by weight, all percentages are by mass percentages, the same as in the following embodiments), mixed in a high-speed mixer for 5 minutes, and then extruded and granulated in a twin-screw extruder with a length-to-diameter ratio of 60:1 and a diameter of 35 mm to obtain a special polypropylene material for frosted cups; the temperatures in each zone of the extruder were: 170°C in zone 1, 180°C in zone 2, 190°C in zone 3, 190°C in zone 4, 185°C in zone 5, and 180°C in the die head.

[0069] The performance test results are shown in Table 2.

[0070] Example 2

[0071] The difference between Example 2 and Example 1 is that the amount of PVCH used in the preparation stage of homopolypropylene is 15g, the amount of mixture A is 0.15g, and 1800g of homopolypropylene is obtained. The other parameters and steps are consistent with Example 1.

[0072] Example 3

[0073] The only difference between Example 3 and Example 1 is that the polymer nucleating agent used is poly-3-methyl-1-butene, and the other parameters and steps are consistent with Example 1, and finally 2000g of homopolypropylene is obtained.

[0074] Example 4

[0075] The only difference between Example 3 and Example 1 is that the polymer nucleating agents used are 5 g each of polyvinyl cyclohexane and poly 3-methyl-1-butene, and the other parameters and steps are consistent with Example 1, and finally 2000 g of homopolypropylene is obtained.

[0076] Comparative Example 1

[0077] The difference between Comparative Example 1 and Example 2 is that 15 g of nucleating agent NA-21 is used instead of PVCH in the preparation stage of homopolypropylene.

[0078] Comparative Example 2

[0079] Preparation of homopolymer polypropylene:

[0080] (1) At 10° C., 1 kg of propylene, 0.25 mL of dicyclopentyldimethoxysilane, 6 mL of triethylaluminum (1 M) and 0.06 g of CS-1 catalyst were sequentially added into a 3 L prepolymerization reactor to carry out propylene prepolymerization for 15 min;

[0081] (2) transferring the propylene prepolymer from the prepolymerization kettle to a 10 L polymerization kettle, adding 17 L of hydrogen and 2 kg of propylene, raising the temperature, and polymerizing the propylene at 70° C. and 3 MPa for 1.5 h to obtain 2100 g of homopolypropylene;

[0082] Processing and granulation: Weigh the materials according to the components and formula provided in Table 1 (Comparative Example 1, adding nucleating agent NA-21), and other conditions are the same as Example 1.

[0083] Comparative Example 3

[0084] The only difference between Comparative Example 3 and Comparative Example 2 is that the nucleating agent added in the granulation stage is PVCH (the type and amount of the nucleating agent are different compared with Comparative Example 2), and the other parameters and steps are consistent with Comparative Example 2.

[0085] Table 1 Components, formulations and processing conditions of the embodiments and comparative examples

[0086]

[0087]

[0088] Table 2 Properties of the materials produced in the examples and comparative examples

[0089]

[0090] Crystallization temperature is a good indicator of the efficiency of the nucleating agent. A higher crystallization temperature means more efficient nucleation in the final product. As can be seen from the data comparison in Table 2, Examples 1 to 4 have higher crystallization temperatures than Comparative Examples 1 to 3, especially Comparative Example 1, indicating that the homopolypropylene provided by the present invention has excellent crystallization properties. Compared with Comparative Example 3 (about 50ppm PVCH), it is shown that the addition of the polymer nucleating agent during the propylene polymerization stage is more uniform in dispersion and has a better nucleation effect.

[0091] The bending modulus characterizes the rigidity of the material. From the data in Table 2, it can be seen that the same amount of polymer nucleating agent is compared with the small molecule nucleating agent (Example 2 and Comparative Example 1), the polymer nucleating agent has a significant rigidity enhancement effect, and 50ppm of the polymer nucleating agent is equivalent to about 1000ppm of the small molecule nucleating agent (Example 2 and Comparative Example 2). Among them, the combination of the two polymer nucleating agents in Example 4 has the best rigidity enhancement effect.

[0092] It can be seen from the heat deformation temperature in Table 2 that the heat deformation temperature of the homopolypropylene prepared by the polymer nucleating agent used in the embodiment of the present invention is significantly higher than that of the comparative example, indicating that the effect of the polymer nucleating agent is significantly better than that of the small molecule nucleating agent at low concentrations.

[0093] It can be seen from the transverse and longitudinal shrinkage data in Table 2 that the transverse and longitudinal shrinkage of the homopolypropylene prepared by the polymer nucleating agent used in the embodiment of the present invention is less than 1.2%, which is significantly better than that of comparative examples 1-3.

[0094] In summary, the present invention provides a high-rigidity, high-heat-resistant and low-shrinkage polypropylene resin and a preparation method thereof. The polypropylene resin prepared by the method has excellent rigidity, heat resistance and dimensional stability.

[0095] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A polypropylene resin composition, characterized in that In parts by weight: 100 parts by weight of a homopolymer polypropylene resin containing a polymer nucleating agent; 0.1-0.3 parts by weight of antioxidant; 0.01-0.1 parts by weight of halogen absorbent; The homopolymer polypropylene resin containing a polymer nucleating agent is prepared by adding a polymer nucleating agent during propylene polymerization; The mass percentage of the polymer nucleating agent in the homopolymerized polypropylene resin containing the polymer nucleating agent is 30 to 50 ppm.

2. The polypropylene resin composition according to claim 1, characterized in that The polypropylene resin composition has a melt index of 10 to 30 g / 10 min at 230° C. / 2.16 kg, a crystallization temperature of more than 125° C., a heat deformation temperature of more than 120° C., and a transverse and longitudinal shrinkage rate of less than 1.2%.

3. The polypropylene resin composition according to claim 1 or 2, characterized in that: The mass percentage of isotactic polypropylene in the homopolymerized polypropylene resin containing a polymer nucleating agent is 98-99.5%.

4. The polypropylene resin composition according to any one of claims 1 to 3, characterized in that The polymer nucleating agent is selected from any one or more of polyvinylcyclopentane, polyvinylcyclohexane, polyvinyl-2-methylcyclohexane, poly-3-methyl-1-butene, poly-3-ethyl-1-hexene, poly-3-methyl-1-pentene or polystyrene; The halogen absorbing agent is selected from any one or more of sodium stearate, calcium stearate or zinc stearate; The antioxidant includes a primary antioxidant and a secondary antioxidant; The primary antioxidant is selected from any one or more of antioxidant 2246, antioxidant 1010, antioxidant 1076 or antioxidant 1330; The auxiliary antioxidant is selected from any one or more of antioxidant 168, antioxidant 626 and antioxidant 9228.

5. The polypropylene resin composition according to claim 4, characterized in that The mass ratio of the main antioxidant to the auxiliary antioxidant is 1:(1-4).

6. A method for preparing a polypropylene resin composition according to any one of claims 1 to 5, characterized in that: include: Adding a polymer nucleating agent during the propylene polymerization process to obtain a homopolymerized polypropylene resin containing the polymer nucleating agent; A homopolymer polypropylene resin containing a polymer nucleating agent, an antioxidant and a halogen absorbent are mixed, extruded and granulated to obtain a polypropylene resin composition.

7. The preparation method according to claim 6, characterized in that: The homopolymer polypropylene resin containing a polymer nucleating agent is prepared according to the following method: S1: prepolymerizing a mixture of a catalyst and a polymer nucleating agent with propylene, an external electron donor, and an alkyl aluminum to obtain a propylene prepolymer; S2: Polymerizing the propylene prepolymer and propylene in the presence of hydrogen to obtain a homopolymerized polypropylene resin containing a polymer nucleating agent.

8. The preparation method according to claim 7, characterized in that: The catalyst is selected from Ziegler-Natta catalysts; The external electron donor is a silane compound, which is selected from vinyl triethoxysilane, vinyl trimethoxysilane, methyl triethoxysilane, dimethyl dimethoxysilane, diethyl dimethoxysilane, dipropyl dimethoxysilane, diisopropyl dimethoxysilane, dibutyl dimethoxysilane, diisobutyl dimethoxysilane, di-tert-butyl dimethoxysilane, di-tert-hexyl dimethoxysilane, diphenyl dimethoxysilane, dicyclohexyl dimethoxysilane, dicyclopentyl dimethoxysilane, dimethyl diethoxysilane, diethyl dieth ... Any one or more of ethoxysilane, diisopropyldiethoxysilane, dibutyldiethoxysilane, diisobutyldiethoxysilane, di-tert-butyldiethoxysilane, di-tert-hexyldiethoxysilane, diphenyldiethoxysilane, dicyclohexyldiethoxysilane, dicyclopentyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, cyclopentylmethyldimethoxysilane, cyclopentyltrimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexyltrimethoxysilane, tert-hexyltrimethoxysilane, tert-butyltrimethoxysilane or tert-hexyltrimethoxysilane; The alkylaluminum is selected from any one or more of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum monochloride, diisobutylaluminum monochloride, dihexylaluminum monochloride or dioctylaluminum monochloride.

9. The preparation method according to any one of claims 6 to 8, characterized in that The prepolymerization temperature in step S1 is -10 to 20°C and the time is 10 to 30 minutes; The polymerization temperature in step S2 is 50-100° C., the pressure is 1-5 MPa, and the time is 1-5 h.

10. A product, characterized in that Made from the polypropylene resin composition according to any one of claims 1 to 5 or the polypropylene resin composition prepared by the preparation method according to any one of claims 6 to 9; The products include automobile parts or home appliance parts.

Citation Information

Cited By

  • Preparation method of polypropylene, polypropylene, low-odor polypropylene resin and preparation method of low-odor polypropylene resin

    CN119708306A

  • A process for the production of polypropylene, polypropylene and low odor polypropylene resin and process for the production thereof

    CN119708306B