Anti-UV aging biodegradable polyester master batch and preparation method thereof

By modifying nano silica and combining with biodegradable polyester resin, a biodegradable polyester masterbatch that resists UV aging is formed, which solves the problem of poor aging performance of existing biodegradable plastics under UV and achieves efficient and long-lasting anti-UV and anti-oxidative aging effects, and reduces preparation costs.

CN118772603APending Publication Date: 2024-10-15INST OF BIOLOGICAL & MEDICAL ENG GUANGDONG ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163216.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing biodegradable plastics have poor aging performance under ultraviolet (UV) light and are prone to yellowing. Commercial light stabilizers have small molecular weight and strong coloring properties, resulting in poor anti-UV effects.

Method used

Use pyrophosphate titanate coupling agent to modify nano silica to form UV-resistant modified nano silica, increase the adsorption strength of UV absorbers, and combine it with biodegradable polyester resin, using phosphoric alcohol hydroxyl groups and epoxy The ring-opening reaction of the groups forms a surface cross-linked network to improve UV absorption and free radical capture capabilities. Combined with antioxidants and hindered amine light stabilizers, biodegradable polyester masterbatch that resists UV aging is prepared.

Benefits of technology

The anti-UV aging performance is improved, the amount of UV absorber is reduced, the migration resistance and low coloration are improved, the toughness and strength of the material are maintained, the service life of the degradable plastic film is extended, and the preparation cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007050680000061
    Figure BDA0005007050680000061
  • Figure BDA0005007050680000062
    Figure BDA0005007050680000062
  • Figure BDA0005007050680000071
    Figure BDA0005007050680000071
Patent Text Reader

Abstract

The invention discloses an anti-UV aging biodegradable polyester master batch and a preparation method thereof.The anti-UV aging biodegradable polyester master batch is prepared from, by mass, 100 parts of biodegradable polyester, 10-20 parts of anti-UV modified nano white carbon black, 3 parts of an antioxidant, 1.5 parts of a chain extender and 2-3 parts of a light stabilizer; firstly, a monomolecular film layer is formed on the surface of nano white carbon black by using a pyrophosphoric acid type titanate coupling agent to adsorb a micromolecular UV absorbent, and then a surface cross-linked network is formed by utilizing a ring-opening reaction of phosphoric acid alcohol hydroxyl and an epoxy group, so that the migration resistance of a UV absorbing group in polyester resin is improved, and the UV absorbing effect is improved. The pyrophosphoric acid type titanate coupling agent has a low-wave-band ultraviolet ray (less than 320 nm) absorption function and a free radical capture function, so that the ultraviolet aging resistance of the master batch is further synergistically improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of plastic materials, and in particular to a UV-resistant biodegradable polyester masterbatch and a preparation method thereof. Background technology:

[0002] At present, biodegradable masterbatch with improved anti-UV aging performance is a granular product made of PBAT, PLA, modified white carbon black, antioxidants, chain extenders and other raw materials through extrusion processing. It has anti-photooxidation and toughening effects. It is mainly used to improve the photoaging service life of biodegradable plastic products. In biodegradable plastic films, it is mainly used to improve the UV aging service life, and can also be used in the production of food packaging bags.

[0003] Biodegradable polyester resin has more photosensitive groups. Adding light stabilizers can solve the problems of poor weather resistance, yellowing, and poor UV and aging resistance of existing plastic products. However, the commercial light stabilizers currently used, especially UV absorbers, have small molecular weights and strong coloring properties. They are easy to migrate and precipitate in polyester, and have poor long-term anti-aging effects. Summary of the invention:

[0004] The purpose of the present invention is to provide a UV-resistant biodegradable polyester masterbatch and a preparation method thereof.

[0005] The present invention is achieved through the following technical solutions:

[0006] The invention discloses a UV aging resistant biodegradable polyester masterbatch. The raw materials include 100 parts of biodegradable polyester, 10-20 parts of UV resistant modified nano-white carbon black, 3 parts of antioxidant, 1.5 parts of chain extender and 2-3 parts of light stabilizer by weight. The UV resistant modified nano-white carbon black is prepared by the following method: 1. a pyrophosphate titanate coupling agent is diluted with a 95% ethanol solution at a weight ratio of 1:1, and then sprayed into the nano-white carbon black powder, stirred at high speed and dried; 2. a UVA absorber and epoxy soybean oil are added to the dried powder, and the mixture is heated, stirred and mixed to obtain the UV resistant modified nano-white carbon black.

[0007] Preferably, the particle size of the modified white carbon black is 20 nm to 200 nm, and the pyrophosphate titanate coupling agent is isopropyl tri(dioctyl pyrophosphate acyloxy) titanate.

[0008] The mass ratio of the nano-white carbon black to the pyrophosphate titanate coupling agent is 100:(1-10).

[0009] The mass ratio of the nano-white carbon black, the UVA absorber and the epoxidized soybean oil is 100:(1-5):(1-5).

[0010] In step ①, the drying temperature is 80-100° C. and the drying time is 0.5-1 h.

[0011] After modifying silica with pyrophosphate titanate coupling agent, the phosphate groups on the surface of silica are increased, the adsorption strength of small molecule UV absorber is enhanced, and the light shielding performance of the material is improved.

[0012] The preferred modified silica can better absorb UV absorbers and, combined with PBAT and PLA, can achieve better anti-light aging effects.

[0013] The biodegradable resin includes one or more of poly(butylene terephthalate-adipate) (PBAT), polylactic acid (PLA), and polypropylene carbonate.

[0014] Preferably, the biodegradable polyester of the present invention uses a certain proportion of poly (butylene terephthalate-adipate) (PBAT) and polylactic acid (PLA) as the base material, and uses a trace amount of chain extender to connect the molecular chains of the two materials to promote the combination of the two base materials, which will not affect the mixed use and reprocessing of the masterbatch with other plastics, and improve the adaptability of the masterbatch to different materials. The prepared masterbatch can be well compatible with the existing degradable plastics, so that the anti-aging components therein can be evenly dispersed in the plastic, thereby achieving a good anti-aging effect, while maintaining the good toughness of the plastic and not reducing the material strength.

[0015] Preferably, the UVA ultraviolet absorber is one or more of 2-hydroxy-4-octyloxybenzophenone (UV-531), β-[3-(2-H-benzotriazole-2-yl)-4-hydroxy-5-tert-butylphenyl]-propionic acid polyethylene glycol 300 ester, and bis-{β-[3-(2-H-benzotriazole-2-yl)-4-hydroxy-5-tert-butylphenyl]-propionic acid}-polyethylene glycol 300 ester.

[0016] Preferably, in the above-mentioned UV aging resistant biodegradable masterbatch, the chain extender is ADR-4468.

[0017] Preferably, in the above-mentioned UV aging resistant biodegradable masterbatch, the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]; a composite antioxidant of pentaerythritol tetrakis(di-T-butyl hydroxyhydrocinnamate) ester (antioxidant 1010) and tris(2,4-di-tert-butyl)phenyl phosphite (antioxidant 168) in a mass ratio of 2:(1-2).

[0018] Preferably, in the above-mentioned UV aging resistant biodegradable masterbatch, the light stabilizer is a hindered amine light stabilizer.

[0019] Preferably, the biodegradable masterbatch with improved UV aging resistance comprises, by weight, 80 parts of poly(butylene terephthalate-adipate), 20 parts of polylactic acid, 10 parts of UV aging-resistant modified white carbon black component, 2 parts of antioxidant 1010, 1 part of antioxidant 168, 1.5 parts of chain extender ADR-4468, and 2 parts of hindered amine 770.

[0020] The preparation method of the UV aging resistant biodegradable polyester masterbatch comprises the following steps: uniformly mixing UV resistant modified nano white carbon black, biodegradable resin, antioxidant, chain extender and light stabilizer, and then extruding and granulating in a twin screw at 120-170°C.

[0021] Preferably, the feed temperature of the extrusion granulation is 120-125°C, and the die temperature is 150-170°C.

[0022] The invention uses nano-white carbon black as a carrier, firstly uses a pyrophosphate titanate coupling agent to hydrolyze and then forms a monomolecular film layer on the surface of the nano-white carbon black to adsorb a small molecule UV absorber, and uses the ring-opening reaction of the phosphate alcohol hydroxyl group and the epoxy group to form a surface cross-linking network, thereby improving the migration resistance of the UV absorbing group in the polyester resin. In the surface structure, the pyrophosphate titanate coupling agent has a low-band ultraviolet (<320nm) absorption function and a free radical capture function, thereby further synergistically improving the anti-ultraviolet aging performance of the masterbatch.

[0023] The beneficial effects of the present invention are as follows:

[0024] 1) The present invention uses a pyrophosphate titanate coupling agent to form a monomolecular film layer on the surface of nano-white carbon black after hydrolysis to adsorb small molecule UV absorbers, and utilizes the ring-opening reaction of phosphate alcohol hydroxyl groups and epoxy groups to form a surface cross-linking network, thereby improving the migration resistance of UV absorbing groups in polyester resins. The pyrophosphate titanate coupling agent has low-band ultraviolet (<320nm) absorption function and free radical capture function, further synergistically improving the anti-ultraviolet aging performance of the masterbatch. Therefore, the anti-UV aging biodegradable masterbatch obtained has a small amount of anti-UV components, is migration-resistant, and has low coloring, and can be directly mixed and dispersed with downstream degradable plastic particles. The preparation method of the anti-aging masterbatch is simple and has low cost.

[0025] 2) The anti-UV aging biodegradable masterbatch obtained by the present invention has high-efficiency and long-lasting anti-ultraviolet and anti-oxidative aging properties. After the prepared degradable plastic film is subjected to ultraviolet accelerated aging for 120 hours, the retention rate of the elongation at break is increased by 2.3 times (comparison between Example 1 and Comparative Example 1), and has a good mechanical property protection effect.

[0026] 3) The anti-UV aging biodegradable masterbatch of the present invention is evenly mixed with the degradable plastic resin, which will not affect the degradable performance of the material. The anti-UV aging biodegradable masterbatch of the present invention is closely connected to the downstream degradable plastic process, and can achieve effective dispersion of the anti-aging additive in the product. The anti-aging masterbatch prepared by the present invention is convenient for use in the post-process, and can be directly mixed with the downstream degradable plastic particles, the process is simple, and the cost is low. Specific implementation method:

[0027] The following is a further description of the present invention, rather than a limitation of the present invention.

[0028] Example 1: Preparation of a UV-resistant biodegradable polyester masterbatch

[0029] 1) 10g of isopropyl tri(dioctyl pyrophosphate) titanate was diluted by half with 95% ethanol, sprayed into 100g of white carbon black powder with a particle size of 20nm, stirred evenly at high speed, dried at 100℃ for 30 minutes, 5g of 2-hydroxy-4-n-octyloxybenzophenone (UV-531) and 5g of epoxy soybean oil were added, stirred at 60℃ for 30 minutes, and mixed evenly to obtain anti-UV modified nano-white carbon black component, and anti-UV modified nano-white carbon black was prepared.

[0030] 2) 80 parts of poly(butylene terephthalate-adipate), 20 parts of polylactic acid, 10 parts of anti-UV aging modified nano-white carbon black component, 1.5 parts of chain extender ADR-4468, 2 parts of hindered amine 770, 2 parts of antioxidant 1010 and 1 part of antioxidant 168 are mixed evenly and extruded into granules by an extrusion granulator. The feed temperature of the extrusion granulation is 120°C and the head temperature is 170°C.

[0031] Example 2: Preparation of a UV-resistant biodegradable polyester masterbatch

[0032] 1) 6g of isopropyl tri(dioctyl pyrophosphate) titanate was diluted with 95% ethanol and sprayed onto 50g of 200nm silica powder and 50g of 20nm silica powder, stirred evenly at high speed, dried at 100°C for 30 minutes, 5g of 2-hydroxy-4-n-octyloxybenzophenone (UV-531) and 3g of epoxy soybean oil were added, stirred at 60°C for 30 minutes, and mixed evenly to obtain an anti-UV modified nano-silica component to prepare an anti-UV modified nano-silica.

[0033] 2) 80 parts of poly(butylene terephthalate-adipate), 20 parts of polylactic acid, 10 parts of anti-UV aging modified nano-white carbon black component, 1.5 parts of chain extender ADR-4468, 2 parts of hindered amine 770, 2 parts of antioxidant 1010 and 1 part of antioxidant 168 are mixed evenly and extruded into granules by an extrusion granulator. The feed temperature of the extrusion granulation is 120°C and the head temperature is 170°C.

[0034] Example 3: Preparation of a UV-resistant biodegradable polyester masterbatch

[0035] 1) 10g of isopropyl tri(dioctyl pyrophosphate) titanate was diluted by half with 95% ethanol, sprayed into 100g of nano-silica powder with a particle size of 20nm, stirred evenly at high speed, dried at 80℃ for 1 hour, 5g of β-[3-(2-H-benzotriazole-2-yl)-4-hydroxy-5-tert-butylphenyl]-propionic acid polyethylene glycol 300 ester and 5g of epoxy soybean oil were added, stirred at 60℃ for 30 minutes, and mixed evenly to obtain anti-UV modified nano-silica component, and anti-UV modified nano-silica was prepared.

[0036] 2) 80 parts of poly(butylene terephthalate-adipate), 20 parts of polylactic acid, 10 parts of anti-UV aging modified nano-white carbon black component, 1.5 parts of chain extender ADR-4468, 2 parts of hindered amine 770, 2 parts of antioxidant 1010 and 1 part of antioxidant 168 are mixed evenly and extruded into granules by an extrusion granulator. The feed temperature of the extrusion granulation is 120°C and the head temperature is 170°C.

[0037] Comparative Example 1:

[0038] The basic composition and preparation method are the same as those in Example 1, except that no UV-resistant modified silica is added.

[0039] Comparative Example 2:

[0040] The basic composition and preparation method are the same as those in Example 1, except that an equal amount of silane coupling agent KH550 is used to replace the isopropyl tri(dioctyl pyrophosphate) titanate to modify the white carbon black.

[0041] Comparative Example 3:

[0042] The basic composition and preparation method are the same as those in Example 1, except that epoxy soybean oil is not used to further crosslink and coat the surface of the silica.

[0043] 3 parts of the masterbatch prepared in each embodiment and comparative example were added to 90 parts of PBAT, 10 parts of PLA and 10 parts of talc respectively, and a plastic film with a thickness of 10 microns was prepared at 170°C, which was cut into 1 cm*10 cm strips and subjected to aging test according to the standards in Table 1. The test results are shown in Table 2:

[0044] Table 1

[0045]

[0046] Table 2:

[0047]

[0048]

Claims

1. A UV-resistant biodegradable polyester masterbatch, characterized in that: The raw materials include 100 parts of biodegradable polyester, 10-20 parts of anti-UV modified nano-white carbon black, 3 parts of antioxidant, 1.5 parts of chain extender, and 2-3 parts of light stabilizer by weight. The anti-UV modified nano-white carbon black is prepared by the following method: ① diluting a pyrophosphate titanate coupling agent with a 95% ethanol solution at a mass ratio of 1:1, spraying the solution into the nano-white carbon black powder, stirring at high speed to evenly mix the solution, and drying the solution; ② Add UVA absorber and epoxy soybean oil to the above dried powder, heat and stir to mix evenly to obtain UV-resistant modified nano-silica.

2. The biodegradable polyester masterbatch according to claim 1, characterized in that: The particle size of the modified white carbon black is 20nm-200nm, and the pyrophosphate titanate coupling agent is isopropyl tri(dioctyl pyrophosphate acyloxy) titanate.

3. The biodegradable polyester masterbatch according to claim 1, characterized in that: The mass ratio of the nano-white carbon black to the pyrophosphate titanate coupling agent is 100:(1-10).

4. The biodegradable polyester masterbatch according to claim 1, characterized in that: The mass ratio of the nano-white carbon black, the UVA absorber and the epoxidized soybean oil is 100:(1-5):(1-5).

5. The biodegradable polyester masterbatch according to claim 1, characterized in that: In step ①, the drying temperature is 80-100° C. and the drying time is 0.5-1 h.

6. The biodegradable polyester masterbatch according to claim 1, characterized in that: The biodegradable resin includes one or more of poly(butylene terephthalate-adipate) (PBAT), polylactic acid (PLA), and polypropylene carbonate; the UVA ultraviolet absorber is one or more of 2-hydroxy-4-n-octyloxybenzophenone (UV-531), β-[3-(2-H-benzotriazole-2-yl)-4-hydroxy-5-tert-butylphenyl]-propionic acid polyethylene glycol 300 ester, and bis-{β-[3-(2-H-benzotriazole-2-yl)-4-hydroxy-5-tert-butylphenyl]-propionic acid}-polyethylene glycol 300 ester.

7. The biodegradable polyester masterbatch according to claim 1, characterized in that: The chain extender is ADR-4468; the light stabilizer is a hindered amine light stabilizer.

8. The biodegradable polyester masterbatch according to claim 1, characterized in that: The antioxidant is a composite antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; pentaerythritol tetrakis(di-T-butyl hydroxyhydrocinnamate) ester and tris(2,4-di-tert-butyl)phenyl phosphite in a mass ratio of 2:(1-2).

9. The biodegradable polyester masterbatch according to claim 1, characterized in that: Calculated by mass, the raw materials include 80 parts of poly(butylene terephthalate-adipate), 20 parts of polylactic acid, 10 parts of anti-UV aging modified white carbon black component, 2 parts of antioxidant 1010, 1 part of antioxidant 168, 1.5 parts of chain extender ADR-4468, and 2 parts of hindered amine 770.

10. The method for preparing the UV-resistant biodegradable polyester masterbatch according to claim 1, characterized in that: The method comprises the following steps: uniformly mixing anti-UV modified nano white carbon black, biodegradable resin, antioxidant, chain extender and light stabilizer, and then extruding and granulating in a twin screw at 120-170 DEG C; the feed temperature of the extrusion granulation is 120-125 DEG C, and the head temperature is 150-170 DEG C.