Binder composition and preparation method thereof, negative pole piece and lithium ion battery

By modifying the branched polyacrylate binder composition, the problem of instability of the electrode sheet caused by the large expansion rate of silicon material in lithium-ion batteries is solved, the transmission efficiency of lithium ions and the cycle stability of the electrode sheet are improved, and the improve the energy density and service life of the battery.

CN118772806APending Publication Date: 2024-10-15ZHEJIANG GEELY HLDG GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410821438.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The silicon material in lithium-ion batteries has a large volume expansion rate during the charge and discharge process, causing the electrode sheet to be unstable and affecting energy density and cycle performance.

Method used

A modified branched polyacrylate binder composition is used to form a branched structure through polymerization reaction, expand the distance between silicon particles, improve lithium ion transmission efficiency, and inhibit the expansion, loosening or falling off of silicon-based materials, and strengthen the electrode sheet cycle stability.

Benefits of technology

It effectively improves the transmission efficiency of lithium ions and the cycle stability of the electrode sheet, extends the service life of the battery, and increases the energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a binder composition and a preparation method thereof, a negative pole piece and a lithium ion battery. The adhesive composition comprises the following components in parts by weight: 50-70 parts of a monofunctional acrylate monomer, 3-15 parts of an acrylate monomer containing a hydrophobic side group with a carbon atom number of 1-18, 1.8-6.4 parts of a polyfunctional acrylate monomer, 0.3-1.5 parts of a free radical initiator, 0.5-1.5 parts of a catalyst and 200-400 parts of a solvent. Therefore, a modified branched polyacrylate binder composition can be obtained through a polymerization reaction, and when the modified branched polyacrylate binder composition and a silicon-based active material are used for preparing slurry, the distance between silicon particles can be enlarged, a smoother transmission channel is provided for lithium ions, and the transmission efficiency of the lithium ions is improved; and the expansion, loosening or falling of the silicon-based material can be effectively inhibited, and the cycling stability of the electrode plate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a binder composition and a preparation method thereof, a negative electrode sheet and a lithium-ion battery. Background Art

[0002] Graphite materials have become the leading product in negative electrode materials for lithium-ion batteries due to their advantages such as high energy density and good cycle performance. However, with the rapid development of lithium-ion batteries, the pursuit of higher energy density is imperative. The theoretical gram capacity of graphite (372mAh / g) has reached its limit, and its energy density has become the key to restricting further breakthroughs in lithium-ion batteries.

[0003] In order to improve the energy density of lithium-ion batteries, silicon materials with higher theoretical gram capacity (~4200mAh / g) have received extensive attention. However, the silicon material itself has a large volume expansion rate during the charging and discharging process, which limits its application. In the lithium battery industry, a more mature solution is to nano-size and carbon-coat the silicon material. As long as the silicon particles are reduced to less than 150nm, the expansion rate will significantly drop from 300% to about 30%. Then the outer layer is carbon-coated, which can act as a buffer layer, thereby further reducing the volume expansion of the silicon-based negative electrode. Composite silicon-based materials such as nano-silicon carbon materials (>1600mAh / g) and silicon oxide (>1200mAh / g) can effectively reduce the expansion of silicon-based negative electrodes, but these materials are often accompanied by unstable factors. For example, incomplete coating or kneading during the homogenization process destroys the coating layer to expose the nano-silicon, which reacts with hydroxide ions to produce gas, resulting in the appearance and initial performance of the electrode sheet being degraded. Summary of the invention

[0004] The present application provides a binder composition and a preparation method thereof, a negative electrode sheet and a lithium ion battery, which can not only improve the cycle stability of the electrode sheet, but also improve the transmission efficiency of lithium ions.

[0005] Specifically, the present application is implemented through the following technical solutions:

[0006] The present application provides a binder composition, comprising the following components:

[0007] A monofunctional acrylate monomer (50 to 70 parts by weight), an acrylate monomer containing a hydrophobic side group having 1 to 18 carbon atoms (3 to 15 parts by weight), a multifunctional acrylate monomer (1.8 to 6.4 parts by weight), a free radical initiator (0.3 to 1.5 parts by weight), a catalyst (0.5 to 1.5 parts by weight) and a solvent (200 to 400 parts by weight).

[0008] Optionally, the binder composition further comprises:

[0009] Acrylic acid monomer (1-9 parts by weight) and / or functional monomer (10-30 parts by weight), wherein the functional monomer comprises at least one of acrylonitrile, acrylamide and sulfonic acid ester.

[0010] Optionally, the binder composition satisfies at least one of the following conditions:

[0011] A. The monofunctional acrylate monomer includes at least one of methyl acrylate, ethyl acrylate and propyl acrylate;

[0012] B. The hydrophobic side groups containing 1 to 18 carbon atoms include at least one of alkanes, substituted alkanes, siloxanes, olefins, aryls and ether groups;

[0013] C. The multifunctional acrylate monomer includes at least one of ethylene glycol diacrylate, hydroxymethyl triacrylate and dipentaerythritol pentaacrylate;

[0014] D. The free radical initiator comprises at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate;

[0015] E. The catalyst comprises at least one metal compound selected from the group consisting of copper oxide, cuprous sulfide, cuprous selenide, cuprous telluride, copper bromide and manganese dioxide;

[0016] F. The solvent is an organic solvent, and the organic solvent includes at least one of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), toluene and acetone;

[0017] G. The weight average molecular weight of the binder composition is 50 w g / mol to 200 w g / mol.

[0018] The present application also provides a method for preparing the binder composition as described above, comprising:

[0019] Firstly, a free radical initiator is added to a solvent, and then a monofunctional acrylate monomer and an acrylate monomer having a hydrophobic side group with 1 to 18 carbon atoms are added to the solvent, and the mixture is reacted at a first temperature for a first time to obtain an intermediate product;

[0020] The multifunctional acrylate monomer and the catalyst are continuously added to the intermediate product, reacted at a second temperature for a second time, and the adhesive composition is obtained by vacuum distillation.

[0021] Optionally, after adding the free radical initiator to the solvent, the method further comprises adding acrylic monomer and / or functional monomer to the solvent;

[0022] Optionally, the first temperature is 60-140° C., and the first time is 2-6 hours; the second temperature is 60-140° C., and the second reaction time is 0.5-2 hours.

[0023] The present application also provides a negative electrode slurry, comprising: an active material containing silicon, a conductive agent, an organic dispersant, an organic solvent and any of the above-mentioned binder compositions;

[0024] The weight ratio of the active material containing silicon element, the conductive agent, the organic dispersant, the organic solvent and the binder composition is (90-98): (0.1-5.0): (0.2-2.0): (100-200): (0.5-10.0).

[0025] Optionally, the negative electrode slurry satisfies at least one of the following conditions:

[0026] H. The conductive agent includes a first conductive agent and a second conductive agent, wherein the first conductive agent includes a granular conductive material, and the second conductive agent includes a tubular conductive material; the weight ratio of the first conductive agent to the second conductive agent is (0.0-2.0): (0.1-3.0);

[0027] I. The organic dispersant includes at least one of polyvinyl pyrrolidone (PVP), a polyether dispersant and a polyester dispersant;

[0028] J. The organic solvent comprises at least one of N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF);

[0029] K. The viscosity of the negative electrode slurry is 2000-6000 cP.

[0030] Optionally, the conductive agent includes a first conductive agent and a second conductive agent, the first conductive agent includes a granular conductive material, and the second conductive agent includes a tubular conductive material;

[0031] The granular conductive material includes at least one of conductive carbon black (SP), Ketjen black, acetylene black, carbon fiber, and graphene (GN); the tubular conductive material includes at least one of single-walled carbon tubes and multi-walled carbon tubes.

[0032] The present application also provides a negative electrode plate, comprising a negative electrode current collector and a coating layer, wherein the coating layer comprises an active material containing silicon and a binder composition as described in any one of the above or a binder composition prepared by any one of the above preparation methods.

[0033] The present application also provides a lithium-ion battery, comprising the negative electrode plate as described above.

[0034] The technical solution provided by this application can achieve the following beneficial effects:

[0035] The present application provides a binder composition and a preparation method thereof, a negative electrode sheet and a lithium-ion battery. The present application can obtain a modified branched polyacrylate binder composition through polymerization reaction, which can not only expand the spacing between silicon particles and provide a smoother transmission channel for lithium ions when preparing slurry with silicon-based active materials, thereby improving the transmission efficiency of lithium ions, but also effectively inhibit the expansion, loosening or shedding of silicon-based materials, thereby improving the cycle stability of the electrode sheet. DETAILED DESCRIPTION

[0036] The technical scheme of the present application will be described in detail below. In the embodiments of the present application, the terms "first", "second" and the like are only used for the purpose of convenience of description and cannot be understood as indicating or implying relative importance. When a numerical range is described in this article, unless otherwise specified, the range is intended to include its end value and all integers and fractions within the range.

[0037] The present application provides a binder composition, comprising the following components:

[0038] A monofunctional acrylate monomer (50 to 70 parts by weight), an acrylate monomer containing a hydrophobic side group having 1 to 18 carbon atoms (3 to 15 parts by weight), a multifunctional acrylate monomer (1.8 to 6.4 parts by weight), a free radical initiator (0.3 to 1.5 parts by weight), a catalyst (0.5 to 1.5 parts by weight) and a solvent (200 to 400 parts by weight).

[0039] The above monomers can be used to obtain a modified branched polyacrylate binder composition through polymerization reaction. When preparing slurry with silicon-based active materials, the improved binder composition has a large number of branching nodes. Compared with the straight-chain linear polyacrylate binder composition, it can not only expand the distance between silicon particles, provide a smoother transmission channel for lithium ions, and improve the transmission efficiency of lithium ions; it also has a branched spatial network structure, which can also form constraints on silicon-based materials, effectively inhibit the expansion, loosening or falling off of silicon-based materials, and improve the cycle stability of the electrode sheet.

[0040] In some embodiments, the binder composition further comprises an acrylic monomer (1 to 9 parts by weight) and / or a functional monomer (10 to 30 parts by weight), wherein the functional monomer comprises at least one of acrylonitrile, acrylamide and sulfonate. Thus, the acrylic monomer can be polymerized into polyacrylic acid (PAA), wherein the carboxyl group can be bonded with the oxygen-containing group on the current collector, such as copper foil, so that the silicon-based active material is better bonded to the surface of the current collector, and the intermolecular force is increased, so as to further effectively inhibit the volume expansion of the silicon-based active material.

[0041] In some embodiments, the adhesive composition further comprises an auxiliary adhesive, wherein the auxiliary adhesive comprises at least one of polyvinylidene fluoride (PVDF), polyimide and polyacrylamide, thereby synergistically improving the adhesion of the adhesive composition.

[0042] In some embodiments, the binder composition satisfies at least one of the following conditions:

[0043] A. The monofunctional acrylate monomer includes at least one of methyl acrylate, ethyl acrylate and propyl acrylate;

[0044] B. The hydrophobic side groups containing 1 to 18 carbon atoms include at least one of alkanes, substituted alkanes, siloxanes, olefins, aryls and ether groups;

[0045] C. The multifunctional acrylate monomer includes at least one of ethylene glycol diacrylate, hydroxymethyl triacrylate and dipentaerythritol pentaacrylate;

[0046] D. The free radical initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate. Thus, the conventional azo free radical initiator can induce the generation of free radical intermediates to allow the monomer molecules to combine with each other.

[0047] E. The catalyst comprises at least one metal compound selected from the group consisting of copper oxide, cuprous sulfide, cuprous selenide, cuprous telluride, copper bromide and manganese dioxide;

[0048] F. The solvent is an organic solvent, and the organic solvent includes at least one of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), toluene and acetone;

[0049] G. The weight average molecular weight of the binder composition is 50 w g / mol to 200 w g / mol.

[0050] The present application also provides a method for preparing the binder composition as described above, comprising:

[0051] Firstly, a free radical initiator is added to a solvent, and then a monofunctional acrylate monomer and an acrylate monomer having a hydrophobic side group with 1 to 18 carbon atoms are added to the solvent, and the mixture is reacted at a first temperature for a first time to obtain an intermediate product;

[0052] The multifunctional acrylate monomer and the catalyst are continuously added to the intermediate product, reacted at a second temperature for a second time, and the adhesive composition is obtained by vacuum distillation.

[0053] Thus, a monofunctional acrylate monomer and an acrylate monomer containing a hydrophobic side group having 1 to 18 carbon atoms can be polymerized first to form a linear long chain structure with a hydrophobic side group, and then continue to polymerize with a multifunctional acrylate monomer to form a network structure, which can effectively inhibit the expansion, loosening or shedding of the silicon-based material and improve the cycle stability of the electrode sheet; in addition, the branched structure of the binder composition obtained by polymerization can also expand the distance between silicon particles, provide a smoother transmission channel for lithium ions, and improve the transmission efficiency of lithium ions.

[0054] In some embodiments, after adding the free radical initiator to the solvent, the method further comprises adding an acrylic monomer and / or a functional monomer to the solvent.

[0055] In some embodiments, the first temperature is 60-140° C., and the first time period is 2-6 hours; the second temperature is 60-140° C., and the second reaction time is 0.5-2 hours.

[0056] The present application also provides a negative electrode slurry, comprising: an active material containing silicon, a conductive agent, an organic dispersant, an organic solvent and any of the above-mentioned binder compositions;

[0057] The weight ratio of the active material containing silicon element, the conductive agent, the organic dispersant, the organic solvent and the binder composition is (90-98): (0.1-5.0): (0.2-2.0): (100-200): (0.5-10.0).

[0058] In some embodiments, the active material containing silicon, i.e., silicon-based material, includes silicon-oxygen material, silicon-carbon material, or silicon composite material. Among them, silicon composite material refers to a mixture of nano-silicon and carbon material, and carbon material includes but is not limited to artificial graphite, natural graphite, mesophase carbon microbeads (MCMB), petroleum coke, carbon fiber, pyrolytic resin carbon, etc.

[0059] Since lithium-ion batteries store and release electrical energy through the movement of lithium ions between the positive and negative electrodes, and during the unlimited charge and discharge process of lithium-ion batteries, the silicon-based active materials continue to expand and contract, which can easily cause cracks and damage on the surface of the silicon-based active materials, causing some lithium ions to be permanently embedded in the gaps, making these lithium ions unable to participate in the subsequent charge and discharge process, resulting in a decrease in the initial capacity of the battery. Therefore, the problem of lithium ion loss can be effectively solved by pre-lithiation of silicon-based active materials to improve the cycle performance of lithium-ion batteries.

[0060] "Pre-lithiation treatment" refers to pre-embedding a portion of lithium ions into silicon-based active materials to compensate for the loss of lithium ions during the initial charging process, thereby achieving a pre-lithiation treatment process for silicon-based active materials. For example, after the electrochemical device is assembled, a pre-charge can be performed to embed a certain amount of lithium ions into the silicon-based active material; for another example, the silicon-based active material can be immersed in a solution containing lithium salts to embed lithium ions into the negative electrode active material.

[0061] In some embodiments, the negative electrode slurry satisfies at least one of the following conditions:

[0062] H. The conductive agent includes a first conductive agent and a second conductive agent, wherein the first conductive agent includes a granular conductive material and the second conductive agent includes a tubular conductive material; the weight ratio of the first conductive agent to the second conductive agent is (0.0-2.0): (0.1-3.0);

[0063] I. The organic dispersant includes at least one of polyvinyl pyrrolidone (PVP), a polyether dispersant and a polyester dispersant;

[0064] J. The organic solvent includes at least one of N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF). In this way, it is possible to avoid the situation in which the nano-silicon is exposed during the homogenization process of the negative electrode slurry of the silicon-based lithium-ion battery due to the kneading action and reacts with the traditional deionized water dispersant to generate gas. The coating effect of the pole piece and the first effect of the battery are improved. The binder composition provided in the present application is used to prepare the negative electrode slurry, which can improve the stability of the slurry, effectively inhibit the pulverization of silicon particles, and improve the cycle stability of silicon-based materials.

[0065] K. The viscosity of the negative electrode slurry is 2000-6000 cP.

[0066] In some embodiments, the conductive agent includes a first conductive agent and a second conductive agent, the first conductive agent includes a granular conductive material, and the second conductive agent includes a tubular conductive material;

[0067] The granular conductive material includes at least one of conductive carbon black (SP), Ketjen black, acetylene black, carbon fiber, and graphene (GN); the tubular conductive material includes at least one of single-walled carbon tubes and multi-walled carbon tubes.

[0068] The present application also provides a negative electrode plate, comprising a negative electrode current collector and a coating layer, wherein the coating layer comprises an active material containing silicon and a binder composition as described in any one of the above or a binder composition prepared by any one of the above preparation methods.

[0069] The present application also provides a lithium-ion battery, comprising the negative electrode plate as described above.

[0070] Taking each weight portion as 10 g as an example, the preparation process of the binder composition, the conductive paste, the negative electrode sheet and the battery cell is described in detail below.

[0071] Example 1

[0072] (1) Preparation of adhesive composition

[0073] To 300 parts by weight of dimethyl sulfoxide (DMSO) in a reaction kettle, 0.9 parts by weight of azobisisobutyronitrile was first added, and then 5 parts by weight of acrylic acid, 60 parts by weight of methyl acrylate, 20 parts by weight of acrylonitrile and 9 parts by weight of octadecyl acrylate were added in sequence, and the mixture was reacted at 80° C. for 4 hours to obtain an intermediate product (A);

[0074]

[0075] 4.1 parts by weight of ethylene glycol diacrylate and 1 part by weight of copper oxide were further added to the intermediate product (A), and the mixture was reacted at 80° C. for 1 hour. The binder composition (B) having a molecular weight of 100 w mol / g was obtained by purification by reduced pressure distillation.

[0076]

[0077] (2) Preparation of conductive paste

[0078] 96 parts by weight of a silicon-based active material (a silicon-carbon composite material obtained by coating the surface of silicon particles with natural graphite), 3 parts by weight of the binder composition obtained in the preparation process (1) above, and 0.9 parts by weight of conductive carbon black (SP) are stirred and mixed to obtain a mixture;

[0079] Then, 30 parts by weight of N-methylpyrrolidone (NMP) and 0.1 parts by weight of oil-based single-walled carbon nanotubes were added to the mixture, stirred and mixed, and the solid content was controlled to 70±10% for full kneading to achieve a uniform dispersion effect; then 0.2 parts by weight of polyvinylpyrrolidone (PVP) and 70 parts by weight of N-methylpyrrolidone (NMP) were used for dilution to obtain a negative electrode slurry with a viscosity of approximately 4500 cP.

[0080] (3) Preparation of negative electrode sheet

[0081] After the negative electrode slurry is filtered through a 100-300 mesh screen, the negative electrode slurry is evenly coated on the front and back sides of the negative electrode current collector copper foil using a coating machine, and the surface density is adjusted to meet the preset (9 mg / cm 2 ) value range, after drying, a semi-finished negative electrode sheet is obtained;

[0082] Then, the semi-finished negative electrode sheet after coating is rolled to a certain thickness by cold roller or oil heated roller to reach the preset compaction density range (1.55mg / cm 3 ), the rolled negative electrode sheet is adjusted to the specified size (length 200 mm, width 50 mm) by a slitting tool or laser cutting to finally obtain the final negative electrode sheet.

[0083] (4) Preparation of battery cells

[0084] Preparation of the positive electrode sheet: 97 parts by weight of positive electrode active material NCM622, 2 parts by weight of polyvinylidene fluoride (PVDF), 1 part by weight of conductive agent carbon nanotubes and 100 parts by weight of N-methylpyrrolidone (NMP) are mixed, coated, rolled and cut to obtain the positive electrode sheet.

[0085] The negative electrode, separator (PP), electrolyte (LiPF6+ethylene carbonate EC / dimethyl carbonate DMC) and aluminum-plastic film are assembled into a test battery cell.

[0086] Example 2

[0087] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, ethylene glycol diacrylate is replaced by hydroxymethyl triacrylate, and the other preparation conditions remain the same as those in embodiment 1. The structural formula of the prepared adhesive composition is shown below.

[0088]

[0089] Example 3

[0090] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, octadecyl acrylate is replaced by perfluorohexadecylethyl acrylate, and the other preparation conditions remain the same as those in embodiment 1. The structural formula of the prepared adhesive composition is shown below.

[0091]

[0092] Example 4

[0093] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, 1.5 parts by weight of azobisisobutyronitrile is first added to 300 parts by weight of dimethyl sulfoxide (DMSO) in a reaction kettle, and then 1 part by weight of acrylic acid, 70 parts by weight of ethyl acrylate, 10 parts by weight of acrylonitrile and 15 parts by weight of octadecyl acrylate are added in sequence, and the mixture is reacted at 80° C. for 4 hours to obtain an intermediate product;

[0094] 6.4 parts by weight of ethylene glycol diacrylate and 1.5 parts by weight of copper oxide were added to the intermediate product, reacted at 80° C. for 1 hour, and purified by vacuum distillation to obtain a binder composition with a molecular weight of 200 w mol / g. The other preparation conditions were the same as those in Example 1.

[0095] Example 5

[0096] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, 0.3 parts by weight of azobisisobutyronitrile is first added to 300 parts by weight of dimethyl sulfoxide (DMSO) in a reaction kettle, and then 9 parts by weight of acrylic acid, 50 parts by weight of methyl acrylate, 30 parts by weight of acrylonitrile and 3 parts by weight of octadecyl acrylate are added in sequence, and the mixture is reacted at 80° C. for 4 hours to obtain an intermediate product;

[0097] 1.8 parts by weight of ethylene glycol diacrylate and 0.5 parts by weight of copper oxide were added to the intermediate product, reacted at 80° C. for 1 hour, and purified by vacuum distillation to obtain a binder composition with a molecular weight of 50 w mol / g. The other preparation conditions were the same as those in Example 1.

[0098] Example 6

[0099] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, 0.9 parts by weight of azobisisobutyronitrile is first added to 300 parts by weight of dimethyl sulfoxide (DMSO) in a reaction kettle, and then 5 parts by weight of acrylic acid, 60 parts by weight of methyl acrylate, 20 parts by weight of acrylonitrile and 9 parts by weight of octadecyl acrylate are added in sequence, and the mixture is reacted at 80° C. for 4 hours to obtain an intermediate product;

[0100] 4.1 parts by weight of ethylene glycol diacrylate and 1 part by weight of copper oxide were further added to the intermediate product, and the mixture was reacted at 80° C. for 0.5 h. The adhesive composition having a molecular weight of about 50 w mol / g was obtained by purification by vacuum distillation. The other preparation conditions were the same as those in Example 1.

[0101] Example 7

[0102] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, 0.9 parts by weight of azobisisobutyronitrile is first added to 300 parts by weight of dimethyl sulfoxide (DMSO) in a reaction kettle, and then 5 parts by weight of acrylic acid, 60 parts by weight of methyl acrylate, 20 parts by weight of acrylonitrile and 9 parts by weight of octadecyl acrylate are added in sequence, and the mixture is reacted at 80° C. for 4 hours to obtain an intermediate product;

[0103] 4.1 parts by weight of ethylene glycol diacrylate and 1 part by weight of copper oxide were further added to the intermediate product, and the mixture was reacted at 80° C. for 2 h. The binder composition having a molecular weight of about 200 w mol / g was obtained by purification by reduced pressure distillation. The other preparation conditions were the same as those in Example 1.

[0104] Example 8

[0105] (4) The difference between this embodiment and embodiment 1 is that in the preparation process (2) of the conductive paste, the silicon-carbon composite material is replaced by silicon monoxide (SiOx) after pre-lithiation treatment. The pre-lithiation treatment process is to mix 100 parts by weight of silicon monoxide (SiOx) and 10 parts by weight of Li2CO3 evenly and then sinter them at 600°C for 4 hours. The other preparation conditions remain the same as in embodiment 1.

[0106] Example 9

[0107] The difference between this embodiment and embodiment 1 is that in the preparation process (1) of the adhesive composition, 0.9 parts by weight of azobisisobutyronitrile is first added to 200 parts by weight of dimethyl sulfoxide (DMSO) in a reaction kettle, and then 60 parts by weight of methyl acrylate and 9 parts by weight of octadecyl acrylate are added in sequence, and the mixture is reacted at 80° C. for 4 hours to obtain an intermediate product;

[0108] 4.1 parts by weight of ethylene glycol diacrylate and 1 part by weight of copper oxide were added to the intermediate product, reacted at 80° C. for 1 hour, and purified by vacuum distillation to obtain a binder composition with a molecular weight of 100 w mol / g. The other preparation conditions were the same as those in Example 1.

[0109] Comparative Example 1

[0110] 96 parts by weight of a silicon-based active material (a silicon-carbon composite material obtained by coating the surface of silicon particles with natural graphite), 3 parts by weight of an aqueous polyacrylate binder, and 0.9 parts by weight of conductive carbon black (SP) were stirred and mixed to obtain a mixture.

[0111] Then, 30 parts by weight of deionized water and 0.1 parts by weight of aqueous single-walled carbon nanotubes were added to the mixture, stirred and mixed, and the solid content was controlled to 70±10% and fully kneaded to achieve a uniform dispersion effect; and then 70 parts by weight of deionized water was used for dilution to obtain a negative electrode slurry with a viscosity of approximately 4500 cP.

[0112] Comparative Example 2

[0113] 96 parts by weight of a silicon-based active material (a silicon-carbon composite material obtained by coating the surface of silicon particles with natural graphite), 3 parts by weight of a polyvinylidene fluoride (PVDF) binder, and 0.9 parts by weight of conductive carbon black (SP) are stirred and mixed to obtain a mixture;

[0114] Then, 30 parts by weight of N-methylpyrrolidone (NMP) and 0.1 parts by weight of aqueous single-walled carbon nanotubes were added to the mixture, stirred and mixed, and the solid content was controlled to 70±10% for full kneading to achieve a uniform dispersion effect; then 0.2 parts by weight of polyvinylpyrrolidone (PVP) and 70 parts by weight of N-methylpyrrolidone (NMP) were used for dilution to obtain a negative electrode slurry with a viscosity of approximately 4500 cP.

[0115] The negative electrode slurries prepared in the above Examples 1-9 and Comparative Examples 1-2 were subjected to static viscosity stability tests, and the cells prepared in the above Examples 1-9 and Comparative Examples 1-2 were subjected to cell first efficiency and fast charge cycle tests, and the test results are shown in Table 1. The specific test methods are as follows:

[0116] Negative electrode slurry static viscosity stability test: After the negative electrode slurry is stirred, the viscosity of the negative electrode slurry is tested at 0 hours, 24 hours, and 48 hours using a rotational viscometer with a speed of 12 rpm in an environment of 25°C ± 3°C, and the viscosity increase rate of 24 hours / 0 hours and 48 hours / 0 hours is calculated.

[0117] Battery cell first efficiency test: In an environment of 25℃±3℃, set the charge and discharge voltage to 2.8~4.5V, the charge and discharge current density to 1C, test the first charge capacity and the first discharge capacity, and calculate the first coulomb efficiency of the battery cell, i.e. the first efficiency, by the first discharge capacity / first charge capacity.

[0118] Fast charge cycle test: In an environment of 25℃±3℃, set the charge and discharge voltage to 2.8~4.5V, the charge current density to 3C, the discharge current density to 1C, the cut-off current to 0.05C, and cycle 100 times according to the above process. Calculate the fast charge cycle capacity retention rate by the discharge capacity at the 100th cycle / the discharge capacity at the 1st cycle.

[0119] Table 1

[0120]

[0121]

[0122] Comparative Example 1 uses deionized water (H2O) as the solvent system. The surface coating of the carbon-based active material is easily destroyed by the kneading effect during the homogenization process, causing the exposed silicon particles to react with the deionized water to produce gas. Comparative Example 2 uses polyvinylidene fluoride (PVDF). Although it has good bonding properties and electrochemical stability, polyvinylidene fluoride is connected to the silicon-based material by weak van der Waals forces, which cannot meet the requirements of drastic volume changes during the charging and discharging process of the silicon-based material, thereby causing the electrode structure to be destroyed, resulting in a rapid attenuation of the electrode capacity, resulting in a low fast charge capacity retention rate.

[0123] The binder composition provided in Examples 1 to 9 of the present application can constrain the silicon-based material to effectively inhibit the expansion, powdering, loosening or falling off of the silicon-based material during the charging and discharging process, and form a coating layer on its surface to reduce the consumption of the electrolyte. At the same time, the steric hindrance provided by the branched structure of the binder composition improves the stability and dispersibility of the slurry. Applying it to the negative electrode slurry can improve the viscosity stability and improve the first effect of the battery. Due to the steric hindrance of the binder composition, it can also ensure a stable ion transmission channel and improve the fast charge cycle capacity retention rate.

[0124] It should be noted that the technical solutions or technical features described in the above embodiments can be combined or supplemented with each other without causing conflicts. The scope of protection of this application is not limited to the precise structures described in the above embodiments; any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of this application should be included in the scope of protection of this application.

Claims

1. A binder composition, characterized in that: Includes the following ingredients: A monofunctional acrylate monomer (50 to 70 parts by weight), an acrylate monomer containing a hydrophobic side group having 1 to 18 carbon atoms (3 to 15 parts by weight), a multifunctional acrylate monomer (1.8 to 6.4 parts by weight), a free radical initiator (0.3 to 1.5 parts by weight), a catalyst (0.5 to 1.5 parts by weight) and a solvent (200 to 400 parts by weight).

2. The adhesive composition according to claim 1, characterized in that The binder composition also includes: Acrylic acid monomer (1-9 parts by weight) and / or functional monomer (10-30 parts by weight), wherein the functional monomer comprises at least one of acrylonitrile, acrylamide and sulfonic acid ester.

3. The adhesive composition according to claim 1, characterized in that At least one of the following conditions is met: A. The monofunctional acrylate monomer includes at least one of methyl acrylate, ethyl acrylate and propyl acrylate; B. The hydrophobic side groups containing 1 to 18 carbon atoms include at least one of alkanes, substituted alkanes, siloxanes, olefins, aryls and ether groups; C. The multifunctional acrylate monomer includes at least one of ethylene glycol diacrylate, hydroxymethyl triacrylate and dipentaerythritol pentaacrylate; D. The free radical initiator comprises at least one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate; E. The catalyst comprises at least one metal compound selected from the group consisting of cupric oxide, cuprous sulfide, cuprous selenide, cuprous telluride, cupric bromide and manganese dioxide; F. The solvent is an organic solvent, and the organic solvent includes at least one of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), toluene and acetone; G. The weight average molecular weight of the binder composition is 50 w g / mol to 200 w g / mol.

4. A method for preparing the binder composition according to any one of claims 1 to 3, characterized in that: include: Firstly, a free radical initiator is added to a solvent, and then a monofunctional acrylate monomer and an acrylate monomer having a hydrophobic side group with 1 to 18 carbon atoms are added to the solvent, and the mixture is reacted at a first temperature for a first time to obtain an intermediate product; The multifunctional acrylate monomer and the catalyst are continuously added to the intermediate product, reacted at a second temperature for a second time, and the adhesive composition is obtained by vacuum distillation.

5. The preparation method according to claim 4, characterized in that: After adding the free radical initiator to the solvent, the method further includes adding acrylic monomer and / or functional monomer to the solvent; And / or, the first temperature is 60-140° C., and the first time is 2-6 hours; the second temperature is 60-140° C., and the second reaction time is 0.5-2 hours.

6. A negative electrode slurry, characterized in that: include: An active material containing silicon, a conductive agent, an organic dispersant, an organic solvent and a binder composition according to any one of claims 1 to 3; The weight ratio of the active material containing silicon element, the conductive agent, the organic dispersant, the organic solvent and the binder composition is (90-98): (0.1-5.0): (0.2-2.0): (100-200): (0.5-10.0).

7. The negative electrode slurry according to claim 6, characterized in that: At least one of the following conditions is met: H. The conductive agent includes a first conductive agent and a second conductive agent, wherein the first conductive agent includes a granular conductive material, and the second conductive agent includes a tubular conductive material; the weight ratio of the first conductive agent to the second conductive agent is (0.0-2.0): (0.1-3.0); I. The organic dispersant includes at least one of polyvinyl pyrrolidone (PVP), a polyether dispersant and a polyester dispersant; J. The organic solvent comprises at least one of N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF); K. The viscosity of the negative electrode slurry is 2000-6000 cP.

8. The negative electrode slurry according to claim 6, characterized in that: The conductive agent includes a first conductive agent and a second conductive agent, wherein the first conductive agent includes a granular conductive material and the second conductive agent includes a tubular conductive material; The granular conductive material includes at least one of conductive carbon black (SP), Ketjen black, acetylene black, carbon fiber, and graphene (GN); the tubular conductive material includes at least one of single-walled carbon tubes and multi-walled carbon tubes.

9. A negative electrode sheet, comprising a negative electrode current collector and a coating layer, characterized in that: The coating layer comprises an active material containing silicon and the binder composition according to any one of claims 1 to 3 or a binder composition prepared by the preparation method according to any one of claims 4 to 5.

10. A lithium ion battery, characterized in that: Comprising the negative electrode sheet as claimed in claim 9.