High-temperature-resistant and high-viscosity pressure-sensitive adhesive and preparation method thereof

By using a combination of copolymer solution, plasticizer and cross-linking agent in the pressure-sensitive adhesive, a tighter network structure is formed, which solves the problem of poor high temperature resistance of the existing pressure-sensitive adhesive and significantly improves its bonding performance and High temperature resistance.

CN118772809AInactive Publication Date: 2024-10-15LINYI QINZHENG COMPOSITE MATERIALS CO LTD

Patent Information

Application Number
CN202410819039.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing acrylic pressure-sensitive adhesives have poor high-temperature resistance, which limits the application fields of pressure-sensitive adhesive products.

Method used

A combination of copolymer solution, plasticizer and cross-linking agent is used to form a tighter network structure through copolymerization and cross-linking reactions to improve bonding performance and high temperature resistance. Specifically, it includes the use of copolymer solution, plasticizer such as dioctyl phthalate, a cross-linker such as aluminum acetylacetonate, and react at a specific temperature.

Benefits of technology

Significantly improves the adhesive performance, cohesive strength and high temperature resistance of pressure-sensitive adhesive, and enhances its mechanical properties and aging resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772809A_ABST
    Figure CN118772809A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant high-viscosity pressure-sensitive adhesive and a preparation method thereof, and relates to the technical field of pressure-sensitive adhesive preparation, the high-temperature-resistant high-viscosity pressure-sensitive adhesive specifically comprises the following raw materials by weight: 80-110 parts of a copolymer solution, 1-5 parts of a plasticizer, 0.8-2.4 parts of a cross-linking agent, and 0.6-1.6 parts of an initiator; wherein the plasticizer is selected from any one of dioctyl phthalate, diisocyanate, phenyl isocyanate, an epoxy organic silicon curing agent 9301 and an isocyanate curing agent 2102. According to the high-temperature-resistant and high-viscosity pressure-sensitive adhesive and the preparation method thereof, by adding the functional monomer, some rigid groups or temperature-resistant groups can be introduced into a polymer by participating in a copolymerization reaction, and the functional monomer has a crosslinkable group, so that a crosslinking site is provided for a further crosslinking reaction; after polymerization, a more compact net structure is formed, so that the adhesion performance of the prepared pressure-sensitive adhesive can be improved, the cohesion strength and the high temperature resistance of the pressure-sensitive adhesive can be improved, and the mechanical property of the pressure-sensitive adhesive can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pressure-sensitive adhesive preparation, in particular to a high-temperature-resistant and high-viscosity pressure-sensitive adhesive and a preparation method thereof. Background Art

[0002] Pressure-sensitive adhesive (PSA) is a soft polymer material with permanent stickiness. It will immediately adhere to the surface of the adhered material with only slight pressure. Pressure-sensitive adhesive is the full name of pressure-sensitive adhesive. It is a type of adhesive that is sensitive to pressure and is mainly used to prepare pressure-sensitive tapes. Its function is to make the tape have pressure-sensitive adhesion properties. Pressure-sensitive adhesive is a special type of adhesive that can be bonded by finger pressure without heating, solvents or other means. Generally, pressure-sensitive adhesive is not used directly for bonding. It must be applied to a strip substrate to make various pressure-sensitive adhesive products before it can be used. Pressure-sensitive adhesive products include pressure-sensitive tapes, pressure-sensitive adhesive label paper, and pressure-sensitive adhesive sheets. Pressure-sensitive tapes are composed of pressure-sensitive adhesive, substrate, primer, back treatment agent, etc. Pressure-sensitive adhesive is the most important component of pressure-sensitive tapes. Its function is to make the tape have pressure-sensitive adhesion properties. The main substrates used are fabrics, plastic films, paper, etc. The primer is to increase the bonding strength between the pressure-sensitive adhesive and the substrate. When in use, tear off the protective film and gently apply pressure to make the tape adhere to the surface of the adherend. The finished products have the following characteristics: bonding can be achieved by finger pressure, and the adhesive does not contaminate the surface of the adherend when tearing off. Among several pressure-sensitive adhesive products, acrylic pressure-sensitive adhesive (APSA) is the most widely used pressure-sensitive adhesive at present, and its usage accounts for more than half of the entire pressure-sensitive adhesive. However, ordinary acrylic pressure-sensitive adhesives have poor high temperature resistance and can only be used at room temperature, which greatly limits the application field of pressure-sensitive adhesive products; for this reason, the present invention provides a high-temperature resistant and high-viscosity pressure-sensitive adhesive and a preparation method thereof. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a high-temperature resistant and high-viscosity pressure-sensitive adhesive and a preparation method thereof, which solves the problems mentioned in the above background technology.

[0004] To achieve the above objectives, the present invention is implemented by the following technical scheme: a high temperature resistant and high viscosity pressure sensitive adhesive, specifically comprising the following raw materials in parts by weight: 80 to 110 parts of copolymer solution, 1 to 5 parts of plasticizer, 0.8 to 2.4 parts of crosslinking agent, and 0.6 to 1.6 parts of initiator; Wherein, the plasticizer is selected from any one of dioctyl phthalate, diisocyanate, phenyl isocyanate, epoxy silicone curing agent 9301 and isocyanate curing agent 2102; and the cross-linking agent is aluminum acetylacetonate.

[0005] Preferably, the initiator is selected from any one of cellulose derivatives, polyacrylamide, gelatin, polyvinyl alcohol, barium sulfate, calcium carbonate, talc, and sodium dodecyl sulfate.

[0006] Preferably, the preparation method of the copolymer solution is: S1, dissolving 4 g of benzoyl peroxide in 80 g of ethyl acetate to obtain a benzoyl peroxide solution for later use; S2, mixing 100 g of the monomer copolymer and 40 g of an ethyl acetate / xylene mixed solvent, heating in a water bath, and stirring; S3, raise the temperature to 75-80°C, add benzoyl peroxide solution dropwise, and keep warm for 1-1.5 hours; S4, continue to add benzoyl peroxide solution, keep warm for 1 to 1.5 hours; S5. Finally, add benzoyl peroxide solution and keep warm for 2 to 2.5 hours.

[0007] Preferably, in S3, the amount of the benzoyl peroxide solution added dropwise is 50%; and in S4 and S5, the amount of the benzoyl peroxide solution added dropwise is both 25%.

[0008] Preferably, the monomer copolymer is composed of a soft monomer, a hard monomer and a functional monomer, wherein the proportions of the monomers are: 45% to 55% of the soft monomer, 40% to 55% of the hard monomer and 1% to 5% of the functional monomer.

[0009] Preferably, the soft monomer is any one or more of isooctyl acrylate and butyl acrylate.

[0010] Preferably, the hard monomer is any one or more of methyl methacrylate, vinyl acetate, and styrene.

[0011] Preferably, the functional monomer is any one of a mixture of methacryloxytrimethoxysilane, trifluoroethyl acrylate and ethoxylated trimethylolpropane triacrylate.

[0012] A method for preparing a high-temperature resistant and high-viscosity pressure-sensitive adhesive comprises the following preparation steps: Step 1, pour 1 / 5 to 1 / 3 of the copolymer solution into the reaction kettle; Step 2: Add initiator, raise the temperature to 80-85°C, and react for 30-60 minutes; Step 3: add the remaining monomer copolymer, plasticizer and cross-linking agent in sequence, mix well, and keep warm at 85-90° C. for 1-3 hours to obtain a high-temperature resistant and high-viscosity pressure-sensitive adhesive.

[0013] The present invention provides a high temperature resistant and high viscosity pressure sensitive adhesive and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects: (1) The high-temperature resistant and high-viscosity pressure-sensitive adhesive and its preparation method can not only introduce some rigid groups or temperature-resistant groups into the polymer by participating in the copolymerization reaction through the addition of functional monomers, but also the functional monomers themselves carry cross-linkable groups, providing cross-linking sites for further cross-linking reactions, and forming a tighter network structure after polymerization, which can not only improve the bonding performance of the prepared pressure-sensitive adhesive, but also improve its cohesive strength and high-temperature resistance, thereby significantly improving its mechanical properties.

[0014] (2) The high-temperature resistant and high-viscosity pressure-sensitive adhesive and its preparation method can enhance the cohesive strength of the pressure-sensitive adhesive by adding a plasticizer and aluminum acetylacetonate, thereby significantly enhancing the high-temperature resistance and aging resistance of the pressure-sensitive adhesive. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A monomer conversion test provided for a high temperature resistant and high viscosity pressure sensitive adhesive and a preparation method thereof of the present invention; Figure 2 The present invention provides a high-temperature resistant and high-viscosity pressure-sensitive adhesive and a preparation method thereof, and provides a photo of the steel plate surface and residual adhesive after a heat resistance test. DETAILED DESCRIPTION

[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] Example 1 A method for preparing a high-temperature resistant and high-viscosity pressure-sensitive adhesive comprises the following preparation steps: Step 1: Pour 16 g of copolymer solution into a reaction kettle; The preparation method of the copolymer solution is as follows: 4 g of benzoyl peroxide is dissolved in 80 g of ethyl acetate to obtain a benzoyl peroxide solution for standby use; 100 g of a monomer copolymer and 40 g of an ethyl acetate / xylene mixed solvent are mixed, heated in a water bath, and stirred; the temperature is raised to 75° C., 36 g of the benzoyl peroxide solution is added dropwise, and the temperature is kept for 1 hour; 36 g of the benzoyl peroxide solution is added dropwise continuously, and the temperature is kept for 1 hour; finally, 18 g of the benzoyl peroxide solution is added dropwise, and the temperature is kept for 2 hours; the composition of the monomer copolymer is: 45% of isooctyl acrylate, 50% of methyl methacrylate, and 5% of methacryloyloxytrimethoxysilane; Step 2: Add 1.6 g of cellulose derivative, heat to 80° C., and react for 30 min; Step 3: add 64 g of monomer copolymer, 5 g of dioctyl phthalate and 2.4 g of aluminum acetylacetonate in sequence, mix well, and keep warm at 85° C. for 1 hour to obtain a high-temperature resistant and high-viscosity pressure-sensitive adhesive.

[0018] Example 2 A method for preparing a high-temperature resistant and high-viscosity pressure-sensitive adhesive comprises the following preparation steps: Step 1, pour 20g of copolymer solution into the reaction kettle; The preparation method of the copolymer solution is as follows: 4 g of benzoyl peroxide is dissolved in 80 g of ethyl acetate to obtain a benzoyl peroxide solution for later use; 100 g of a monomer copolymer and 40 g of an ethyl acetate / xylene mixed solvent are mixed, heated in a water bath, and stirred; the temperature is raised to 75° C., 36 g of the benzoyl peroxide solution is added dropwise, and the temperature is kept for 1.5 hours; 36 g of the benzoyl peroxide solution is added dropwise continuously, and the temperature is kept for 1 hour; finally, 18 g of the benzoyl peroxide solution is added dropwise, and the temperature is kept for 2.5 hours; the composition of the monomer copolymer is: 50% of butyl acrylate, 48% of vinyl acetate, and 2% of a mixture of trifluoroethyl acrylate and ethoxylated trimethylolpropane triacrylate; Step 2: Add 1.1 g of polyacrylamide, heat to 85°C, and react for 45 minutes; Step 3: add 80g of monomer copolymer, 3g of diisocyanate and 1.6g of aluminum acetylacetonate in sequence, mix well, and keep warm at 90°C for 2h to obtain a high-temperature resistant and high-viscosity pressure-sensitive adhesive.

[0019] Example 3 A method for preparing a high-temperature resistant and high-viscosity pressure-sensitive adhesive comprises the following preparation steps: Step 1, pour 22g of copolymer solution into a reaction kettle; The preparation method of the copolymer solution is as follows: 4 g of benzoyl peroxide is dissolved in 80 g of ethyl acetate to obtain a benzoyl peroxide solution for standby use; 100 g of a monomer copolymer and 40 g of an ethyl acetate / xylene mixed solvent are mixed, heated in a water bath, and stirred; the temperature is raised to 80° C., 36 g of the benzoyl peroxide solution is added dropwise, and the temperature is kept for 1.5 hours; 36 g of the benzoyl peroxide solution is added dropwise continuously, and the temperature is kept for 1.5 hours; finally, 18 g of the benzoyl peroxide solution is added dropwise, and the temperature is kept for 2.5 hours; the composition of the monomer copolymer is: 55% of butyl acrylate, 44% of styrene, and 1% of methacryloyloxytrimethoxysilane; Step 2: Add 0.6 g of sodium dodecyl sulfate, raise the temperature to 85°C, and react for 60 minutes; Step 3: add 88g of monomer copolymer, 1g of epoxy silicone curing agent 9301 and 0.8g of aluminum acetylacetonate in sequence, mix well, and keep warm at 90°C for 3h to obtain a high-temperature resistant and high-viscosity pressure-sensitive adhesive.

[0020] Comparative Example 1 A method for preparing a high-temperature resistant and high-viscosity pressure-sensitive adhesive comprises the following preparation steps: Step 1: Pour 16g of monomer copolymer into a reaction kettle, wherein 45% isooctyl acrylate, 50% methyl methacrylate, and 5% methacryloyloxytrimethoxysilane; Step 2: Add 1.6 g of cellulose derivative, heat to 80° C., and react for 30 min; Step 3: add 64 g of the monomer copolymer and 2.4 g of aluminum acetylacetonate in sequence, mix well, and keep warm at 85° C. for 1 hour to obtain a high-temperature resistant and high-viscosity pressure-sensitive adhesive.

[0021] Monomer conversion test: Place the aluminum foil, weigh its mass as m1, add 2 drops of 2.0wt% hydroquinone solution, dry in a vacuum oven at 150℃ for 12h, weigh its mass as m2; the results are as follows Figure 1 As shown; the calculation formula of the solid content S of the sample is: ; The calculation formula of monomer conversion rate C is: ;Wherein, G is the theoretical solid content.

[0022] Depend on Figure 1 It can be seen that in the present technical solution, the conversion rate of the monomer is improved, and as the reaction time increases, the conversion rate of the monomer shows an upward trend, which effectively reduces the residual monomer.

[0023] Sample preparation: Use a coating rod to coat the pressure-sensitive adhesive on a 50mm PET film, dry it at 110℃ for 3min, take out the release film, control the dry thickness of the adhesive layer to 9~10μm, and finally place it in an oven at 40℃ for 48h.

[0024] Performance Test: Adhesion performance test: (1) Initial adhesion: tested according to GB / T4852-2002, with a slope angle of 30° and a sample size of 24 mm × 55 mm; (2) Adhesion test: The test is conducted in accordance with GB / T 4851-2014 "Test method for adhesion of adhesive tapes". The sample is attached to the sample plate, pressed back and forth 15 times with a 2kg handwheel, and then hung vertically on the test frame. A 1kg weight is hung at the lower end, and the time it takes for the sample to completely detach is recorded. The sample size is 50mm × 100mm. (3) 180° peel strength: Referring to GB / T2792-2014 standard, the bonding time between the tape and the steel plate was set to 2 h, and the test was carried out using a microcomputer-controlled annular peel strength tester; the sample size was 24 mm × 250 mm; the results are shown in Table 1: Table 1 It can be seen from Table 1 that the adhesive holding force and 180° peel strength of the pressure-sensitive adhesive prepared in the present application are significantly enhanced, thereby improving the comprehensive performance of the pressure-sensitive adhesive.

[0025] Heat resistance test: The sample was bonded to a steel plate and placed in an oven at 100°C for 8 hours according to GB / T 2792-2014. After being taken out, it was naturally cooled to room temperature. After peeling off, the glass surface was observed for any residual adhesive. The sample size was 40mm × 40mm. The results were as follows: Figure 2 As shown: the pressure-sensitive adhesive prepared by the technical solution has no residual adhesive and its heat resistance is significantly improved.

[0026] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0027] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0028] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high temperature resistant and high viscosity pressure sensitive adhesive, characterized in that: Specifically, the raw materials include the following parts by weight: 80-110 parts of copolymer solution, 1-5 parts of plasticizer, 0.8-2.4 parts of crosslinking agent, and 0.6-1.6 parts of initiator; Wherein, the plasticizer is selected from any one of dioctyl phthalate, diisocyanate, phenyl isocyanate, epoxy silicone curing agent 9301 and isocyanate curing agent 2102; and the cross-linking agent is aluminum acetylacetonate.

2. A high temperature resistant and high viscosity pressure sensitive adhesive according to claim 1, characterized in that: The initiator is selected from any one of cellulose derivatives, polyacrylamide, gelatin, polyvinyl alcohol, barium sulfate, calcium carbonate, talc, and sodium dodecyl sulfate.

3. The high temperature resistant and high viscosity pressure sensitive adhesive according to claim 1, characterized in that: The preparation method of the copolymer solution is: S1, dissolving 4 g of benzoyl peroxide in 80 g of ethyl acetate to obtain a benzoyl peroxide solution for later use; S2, mixing 100 g of the monomer copolymer and 40 g of an ethyl acetate / xylene mixed solvent, heating in a water bath, and stirring; S3, raise the temperature to 75-80°C, add benzoyl peroxide solution dropwise, and keep warm for 1-1.5 hours; S4, continue to add benzoyl peroxide solution, keep warm for 1 to 1.5 hours; S5. Finally, add benzoyl peroxide solution and keep warm for 2 to 2.5 hours.

4. A high temperature resistant and high viscosity pressure sensitive adhesive according to claim 3, characterized in that: In S3, the amount of the benzoyl peroxide solution added dropwise is 50%; in S4 and S5, the amount of the benzoyl peroxide solution added dropwise is both 25%.

5. The high temperature resistant and high viscosity pressure sensitive adhesive according to claim 3, characterized in that: The monomer copolymer is composed of a soft monomer, a hard monomer and a functional monomer, wherein the proportions of the monomers are: 45% to 55% of the soft monomer, 40% to 55% of the hard monomer and 1% to 5% of the functional monomer.

6. A high temperature resistant and high viscosity pressure sensitive adhesive according to claim 5, characterized in that: The soft monomer is any one or more of isooctyl acrylate and butyl acrylate.

7. The high temperature resistant and high viscosity pressure sensitive adhesive according to claim 5, characterized in that: The hard monomer is any one or more of methyl methacrylate, vinyl acetate and styrene.

8. The high temperature resistant and high viscosity pressure sensitive adhesive according to claim 5, characterized in that: The functional monomer is any one of a mixture of methacryloxytrimethoxysilane, trifluoroethyl acrylate and ethoxylated trimethylolpropane triacrylate.

9. A method for preparing a high temperature resistant and high viscosity pressure sensitive adhesive according to any one of claims 1 to 8, characterized in that: The method comprises the following preparation steps: Step 1, pour 1 / 5 to 1 / 3 of the copolymer solution into the reaction kettle; Step 2: Add initiator, raise the temperature to 80-85°C, and react for 30-60 minutes; Step 3: add the remaining monomer copolymer, plasticizer and cross-linking agent in sequence, mix well, and keep warm at 85-90° C. for 1-3 hours to obtain a high-temperature resistant and high-viscosity pressure-sensitive adhesive.

Citation Information

Patent Citations

  • Adhesive agent and adhesive sheet

    JP2021102674A

Cited By

  • Single-component acrylate pressure-sensitive adhesive and preparation method thereof

    CN119614109A