Blue-light-excited Mn < 4 + >-doped red light material and preparation method thereof

The blue-light-excited Mn4+-doped fluorooctate red luminescent material is synthesized by solid-phase method, which solves the problem of using toxic hydrofluoric acid in the traditional method, realizes green chemical synthesis and efficient production, and is suitable for the red light emission of blue LED chips. , demonstrating excellent luminescence performance and stability.

CN118772886APending Publication Date: 2024-10-15YUNNAN MINZU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410970264.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional synthesis of Mn4+-activated fluoride phosphors uses toxic hydrofluoric acid, which results in high production costs, poor chemical stability, and difficulty in accurately controlling the content of Mn4+ ions, resulting in waste of raw materials and potential safety hazards.

Method used

The blue-light-excited Mn4+-doped fluorooctate red luminescent material Cs2RbY1-xF6:xMn4+ was synthesized using a solid-phase method. Through the ammonium salt-assisted synthesis method, the use of toxic HF reagents was avoided, the reaction conditions were controlled, and automated production and efficient raw material utilization were achieved.

Benefits of technology

It achieves green chemical synthesis, reduces production costs and labor costs, avoids waste of raw materials, is suitable for large-scale industrial production, and shows excellent luminescence performance and stability, and is suitable for red light emission of blue LED chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772886A_ABST
    Figure CN118772886A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of luminescent material synthesis, and discloses blue light excited Mn < 4 + > doped yttrium fluoride red fluorescent powder and a preparation method thereof, the chemical composition of the red fluorescent powder material is Cs2RbY (1-x) F6: xMn < 4 + >, x is the molar percentage coefficient of Mn < 4 + > doped ions relative to Y < 3 + > ions, and x is more than or equal to 0.3% and less than or equal to 1.5%. The excitation wavelength of the blue light is 450-480 nm, the red fluorescent material can obtain a series of narrow-band emission peaks under the excitation of the blue light, and the v6 peak intensity of about 628 nm is the highest. The preparation method of the red fluorescent material is an ammonium salt assisted synthesis low-temperature solid-phase method, is carried out at 70-120 DEG C, is simple in process, low in cost and low in energy consumption, does not use a harmful substance HF, and is very suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of luminescent material synthesis technology, and specifically relates to a blue light excited Mn 4+ Doped red light emitting material and preparation method thereof. Background Art

[0002] Mn 4+ Activated fluoride has the advantages of low preparation cost, good chemical stability and excellent optical properties, and is considered to be one of the most promising candidate materials for red phosphors. 4+ Activated fluoride can generate high-purity red light around 630 nm under the excitation of ultraviolet-blue light (300 ~ 550nm), which matches well with the emission wavelength of blue LED chips (such as GaN chips). However, the use of toxic hydrofluoric acid in traditional synthesis methods has hindered its development and commercialization.

[0003] Mn 4+ Activated fluoride phosphors are usually synthesized by wet chemical methods, in which hydrofluoric acid is used as a fluoride source. Unfortunately, HF solutions are highly volatile and toxic, posing serious risks to the skin, eyes, and bones of operators even at low exposure levels. In addition, since some Mn 4+ ions, Mn cannot be accurately controlled 4+ The liquid phase method often uses excessive reactants to ensure the integrity of the reaction, which may lead to a waste of raw materials. Therefore, it is necessary to develop a new green method to effectively synthesize Mn-doped 4+ Fluoride phosphor. Summary of the invention

[0004] In order to solve the above problems, the present invention uses a solid phase method to synthesize Mn under blue light excitation 4+ Doped fluoroyttrium red luminescent material Cs 2 Yj Y 1-x F 6 :xMn 4+ , x is the corresponding doped Mn 4+ Ion relative to Y 3+The molar percentage coefficient of the ion is 0.3% ≤ x ≤ 1.5%. The red luminescent material is excited by blue light (450 ~ 480 nm) to produce a series of narrow-band emission peaks in the red light band, among which the strongest emission peak is near 628 nanometers. The red light material is prepared by the solid phase method, which is a relatively direct and simple grinding process. The preparation conditions are easy to control, the waste of raw materials is small, and it is suitable for large-scale production. Its advantage is that the whole process does not require the use of toxic and corrosive HF reagents, and can realize automated production, improve production efficiency, and reduce labor costs. It is very consistent with the principles of green chemistry and is suitable for large-scale industrial production. In addition, the solid phase method does not require the use of excessive reactants to ensure the integrity of the reaction, avoiding the waste of raw materials.

[0005] Specifically, the present invention uses the solid phase method of ammonium salt-assisted synthesis to prepare the above-mentioned red light material. On the one hand, the ammonium salt-assisted synthesis can provide fluorine elements for the synthesis of the material without introducing new impurity elements. On the other hand, the Cs 2 Yb 6 For the raw materials involved in the reaction, ammonium salt can also be used in excess to allow other raw materials to react fully, and excess ammonium salt will directly decompose as the temperature rises during the reaction.

[0006] On the other hand, the present invention also provides a blue light excited Mn 4+ The preparation method of the doped red light material comprises the following steps: Step 1, add cesium carbonate, rubidium carbonate, yttrium trioxide, ammonium hydrogen fluoride, and cesium hexafluoromanganate into a polytetrafluoroethylene mortar and grind until the color is evenly distributed; Step 2, adding anhydrous ethanol, grinding, and placing in a vacuum drying oven to dry; Step 3: Add anhydrous ethanol again, grind, and dry in a vacuum drying oven to obtain a yellow powder as the final product.

[0007] Furthermore, in step 1, the mass percentages of cesium carbonate, rubidium carbonate, yttrium trioxide, ammonium hydrogen fluoride and cesium hexafluoromanganate are 44.5-44.8%, 15.7-15.9%, 15.4-15.5%, 23.3-23.8% and 0.17-0.87%, respectively.

[0008] Furthermore, in step 2 and step 3, the temperature of the vacuum drying oven is 70-120°C.

[0009] Furthermore, in steps 2 and 3, the drying time in the vacuum drying oven is 3 to 5 hours.

[0010] Beneficial effects of the present invention: The red fluorescent material involved in the present invention has simple process, low cost, low energy consumption, and does not use harmful substances HF, and is very suitable for large-scale industrial production. In addition, the fluorescent powder prepared by the present invention is similar to Y 3 Al 5 O 12 :Ce 3+ The yellow phosphor is mixed and packaged on the GaN blue light chip, showing excellent luminescence properties such as color temperature: 3504 K and color rendering index: 91.3. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 Cs in Example 1 2 Yb 6 :0.9%Mn 4+ Scanning electron microscope image of red phosphor.

[0012] Figure 2 Cs in Example 1 2 Yb 6 :xMn 4+ XRD diffraction patterns of (x = 0.3%, 0.6%, 0.9%, 1.2%, 1.5%); Figure 3 Cs in Example 1 2 Yb 6 :0.9%Mn 4+ EDS spectrum of Figure 4 Cs in Example 1 2 Yb 6 :xMn 4+ Excitation spectra of (x = 0.3%, 0.6%, 0.9%, 1.2%, 1.5%) (monitoring wavelength is 628 nm); Figure 5 Cs in Example 1 2 Yb 6 :xMn 4+ Emission spectra of (x = 0.3%, 0.6%, 0.9%, 1.2%, 1.5%) (excitation wavelength is 473 nm), the inset is the normalized trend diagram of luminescence intensity; Figure 6 Cs in Example 1 2 Yb 6 :0.9%Mn 4+ Emission spectra of phosphors at different temperatures; the illustration is the normalized trend graph of luminescence intensity at different temperatures; Figure 7 is Cs in Example 1 under 20 mA current excitation 2 Yb 6:0.9%Mn 4+ Electroluminescence spectrum of phosphors; Figure 8 is Cs under different current excitation in Example 1 2 Yb 6 :0.9%Mn 4+ Electroluminescence spectrum of phosphor. DETAILED DESCRIPTION

[0013] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and examples.

[0014] 0.8144 g of cesium carbonate (Cs 2 CO 3 ), 0.2885 g of rubidium carbonate (Rb 2 CO 3 ), 0.2823 g yttrium trioxide (Y 2 O 3 )、0.4278 g ammonium hydrogen fluoride ((NH 4 )HF 2 ), 0.0032 g cesium hexafluoromanganate (Cs 2 Mn 6 ) was added to a polytetrafluoroethylene mortar and ground until the color was uniform. A small amount of anhydrous ethanol was added to the ground sample, ground, and placed in a 70°C vacuum drying oven for 3 hours. The dried sample was once again ground with anhydrous ethanol and dried for another 3 hours to obtain a yellow powder, which was Cs 2 Yb 6 :Mn 4+ Red phosphor final product. Figure 1 It's Cs 2 Yb 6 :0.9%Mn 4+ Scanning electron microscope image of red phosphor. Figure 1 It can be seen that Cs 2 Yb 6 :0.9%Mn 4+ The powder particles have good dispersibility, and most of them are octahedral in shape, which indicates that Mn 4+ Doping into Cs 2 Yb 6 In the microscopic structure, there is a tendency to form an octahedral luminescent particle center with a small size of 10 microns.

[0015] Different Mn 4+ Cs doping concentration 2 Yb 6 :Mn 4+ The XRD diffraction pattern of red phosphor is as follows Figure 2 The diffraction peaks of all samples are completely matched with the data of standard card 04-001-8106, which indicates that Cs 2 Yb 6 A single pure phase also indicates a small amount of Mn 4+ The doping of Mn does not change the phase purity of the material, which is conducive to exploring 4+ Ion doping into Cs 2 Yb 6 Study on the luminescence properties brought by the structure. Figure 3 Yes Cs 2 Yb 6 :0.9%Mn 4+ The EDS spectrum test of the red phosphor was carried out. The EDS spectrum confirmed the Cs, Rb, Y, F, and Mn elements of the phosphor. The Au element was due to the need for gold plating during the measurement. No other impurity elements were observed in the sample, which further proved that Cs was successfully synthesized. 2 Yb 6 The matrix, and Mn 4+ successfully doped into the lattice. In addition, Figure 3 The illustration shows the percentage of each element, where the atomic content roughly satisfies Cs:Rb:Y:F = 2:1:1:6, which is consistent with Cs 2 Yb 6 The stoichiometric ratios of the individual atoms of the matrix are matched.

[0016] Figure 4 and Figure 5 The samples are shown in Figure 2 for different Mn 4+ The excitation spectrum (monitoring wavelength is 628 nm) and emission spectrum (excitation wavelength is 473 nm) of the doping concentration. The luminescence intensity shows a trend of increasing first and then decreasing with the increase of doping concentration. In particular, when x = 0.9%, Cs 2 Yb 6 :0.9%Mn 4+ The excitation and emission spectra of the phosphor reach their strongest intensities. Figure 5 The illustration is a normalized trend diagram of the luminescence intensity under different gradients, which shows the changing trend of the luminescence intensity more clearly. The sample has two strong broadband excitations in the ultraviolet light region (320 ~ 390 nm) and the blue light region (400 ~ 500 nm). The two broad excitation bands correspond to Mn 4+ of 4 A 2g → 4 T 1g and 4 A 2g → 4 T2g The strongest excitation peak is located at about 473 nm. Under the excitation of 450 ~ 480 nm blue light, the emission of the sample is a series of narrow-band emission spectra, belonging to Mn 4+ The strongest emission peak is around 628 nm. In particular, at room temperature, Cs 2 Yb 6 :0.9%Mn 4+ The CIE coordinate values ​​of the phosphor emission spectrum are: x = 0.686, y = 0.314; the color purity is 98.8%.

[0017] Figure 6 Cs 2 Yb 6 :0.009Mn 4+ The emission spectra of phosphors at different temperatures, such as Figure 6 As shown, as the temperature increases, the seven characteristic peaks of the phosphor are almost in the same position and similar in shape, which shows that the phosphor of the present invention has good stability and will not decompose as the temperature increases. In addition, Figure 6 The illustration is a normalized trend diagram of luminescence intensity at different temperatures, which can more clearly show the intensity changes of the emission spectrum at different temperatures.

[0018] Figure 7 The figure shows that under 20 mA current excitation, Cs 2 Yb 6 :0.9%Mn 4+ Phosphors and Commercial YAG:Ce 3+ Electroluminescence spectrum of warm white LED device made of yellow phosphor and blue LED chip. The blue light emission peak at 460 nm originates from the emission of GaN chip, and the emission peak in the range of 500 nm to 600 nm originates from YAG:Ce 3+ The color temperature of this white light LED device is 3504 K and the color rendering index is 91.3. Figure 8 The variable current electroluminescence spectrum of the white light LED device was tested under different current driving conditions of 20 ~ 180 mA. It can be concluded that the emission intensity shows an increasing trend with the increase of driving current, and no saturation phenomenon occurs. The above results show that Cs 2 Yb 6 :0.9%Mn 4+ It can be used as a high-efficiency red light component in WLEDs devices and has good application prospects in the lighting field of new warm WLEDs devices.

[0019] Based on Example 1, 0.8144 g of Cs 2 CO 3, 0.2885 g of Rb 2 CO 3 , 0.2823 g Y 2 O 3 , 0.4192 g (NH 4 )HF 2 , 0.0064 g Cs 2 Mn 6 Add it to a polytetrafluoroethylene mortar and grind it until the color is uniform. Add a small amount of anhydrous ethanol to the ground sample, grind it, and place it in a 90℃ vacuum drying oven to dry for 4 hours. After drying, add anhydrous ethanol to the sample again, grind it, and dry it for another 4 hours to obtain a yellow powder, which is Cs 2 Yb 6 : Mn 4+ Red phosphor final product.

[0020] Based on Example 1, 0.8062 g of Cs 2 CO 3 , 0.2885 g of Rb 2 CO 3 , 0.2794 g Y 2 O 3 , 0.4278 g (NH 4 )HF 2 , 0.0064 g Cs 2 Mn 6 Add it to a polytetrafluoroethylene mortar and grind it until the color is uniform. Add a small amount of anhydrous ethanol to the ground sample, grind it, and place it in a 120 ℃ vacuum drying oven to dry for 5 hours. After drying, add anhydrous ethanol to the sample again, grind it, and dry it for another 5 hours to obtain a yellow powder, which is Cs 2 Yb 6 : Mn 4+ Red phosphor final product.

[0021] Based on Example 1, 0.8144 g of Cs 2 CO 3 , 0.2856 g of Rb 2 CO 3 , 0.2794 g Y 2 O 3 , 0.4278 g (NH 4 )HF 2 , 0.0064 g Cs 2 Mn 6Add it to a polytetrafluoroethylene mortar and grind it until the color is uniform. Add a small amount of anhydrous ethanol to the ground sample, grind it, and place it in a 120 ℃ vacuum drying oven to dry for 5 hours. After drying, add anhydrous ethanol to the sample again, grind it, and dry it for another 5 hours to obtain a yellow powder, which is Cs 2 Yb 6 : Mn 4+ Red phosphor final product.

[0022] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A blue light excited Mn 4+ The doped red light emitting material is characterized by: Its chemical formula is Cs2RbY 1-x F6:xMn 4+ , x is Mn 4+ Doping ions relative to Y 3+ The molar percentage coefficient of the ion is 0.3% ≤ x ≤ 1.5%.

2. The blue light excited Mn as claimed in claim 1 4+ The doped red light emitting material is characterized by: The blue light excitation wavelength is 450-480 nm.

3. The blue light excited Mn as claimed in claim 1 4+ The doped red light emitting material is characterized by: The red light material is prepared by a solid phase method assisted by ammonium salt synthesis.

4. The blue light excited Mn as claimed in claim 1 4+ The method for preparing a doped red light material is characterized in that: The steps include: Step 1, add cesium carbonate, rubidium carbonate, yttrium trioxide, ammonium hydrogen fluoride, and cesium hexafluoromanganate into a polytetrafluoroethylene mortar and grind until the color is evenly distributed; Step 2, adding anhydrous ethanol, grinding, and placing in a vacuum drying oven to dry; Step 3: Add anhydrous ethanol again, grind, and dry in a vacuum drying oven to obtain a yellow powder as the final product.

5. The blue light excited Mn as claimed in claim 4 4+ The method for preparing a doped red light material is characterized by: In step 1, the mass percentages of cesium carbonate, rubidium carbonate, yttrium trioxide, ammonium hydrogen fluoride and cesium hexafluoromanganate are 44.5-44.8%, 15.7-15.9%, 15.4-15.5%, 23.3-23.8% and 0.17-0.87%, respectively.

6. The blue light excited Mn as claimed in claim 5 4+ The method for preparing a doped red light material is characterized by: In step 2 and step 3, the temperature of the vacuum drying oven is 70 to 120°C.

7. The blue light excited Mn as claimed in claim 6 4+ The method for preparing a doped red light material is characterized by: In steps 2 and 3, the drying time in the vacuum drying oven is 3 to 5 hours.

Citation Information

Patent Citations

  • Synthesis method of ytterbium and thulium doped fluoride used for up-conversion white light

    CN105112051A

  • Tetravalent manganese ion and chromium ion co-doped scandium-based fluoride broadband near-infrared luminescent material and preparation method thereof

    CN116463121A

  • Na3ScF6 and preparation method thereof

    CN117534111A