Method for comprehensively utilizing sulfuric-acid residues

By pressing sulfuric acid slag into briquettes as converter cold material, the converter process is used to efficiently recover iron, cobalt, nickel, and zinc elements, which solves the problems of low utilization efficiency and environmental pollution of sulfuric acid slag in the existing technology, and achieves cost reduction and resource reduction. efficient utilization.

CN118773445APending Publication Date: 2024-10-15ZHONGHUA GEOLOGY MINE ZONGJU GEOLOGY RES YUAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908181.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing comprehensive utilization technology of sulfuric acid slag requires pyrometallurgy, magnetic separation or chemical leaching. The process is long and has sulfur emission problems, which increases the investment cost and makes it difficult to efficiently utilize the iron, cobalt, nickel and zinc elements in the sulfuric acid slag.

Method used

The sulfuric acid slag is ground and graded, then water and binder are added and pressed into briquettes, which are used as converter cold materials. The converter process is used to efficiently recover iron, cobalt, nickel, and zinc elements, and metallic zinc is obtained through molten iron reduction. .

Benefits of technology

It achieves efficient recycling of sulfuric acid slag, reduces steelmaking costs, solves environmental pollution problems, and achieves the purpose of reducing costs and increasing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of chemical metallurgy, and particularly discloses a comprehensive utilization method of sulfuric-acid slag. The method comprises the following steps: grinding sulfuric-acid residues, carrying out size fraction matching, adding water and a binder into the matched material, pressing into a block mass, and preparing into a dry block mass; feeding the dry block mass into a converter to be used as a cold material; the particle size matching mode is as follows: 10-20% of materials of which the particle sizes are more than 0.3 mm and less than or equal to 0.5 mm; materials of which the particle sizes are more than 0.045 mm and less than or equal to 0.3 mm account for 20-40%; the material with the particle size of less than or equal to 0.045 mm accounts for 40-70%; adding water to enable the water content of the matched materials to be 7.5-8.0%; the addition amount of the binder accounts for 3-5% of the weight percentage of the matched materials. The process characteristics of the converter are utilized, the sulfuric-acid residues are pressed into the block mass to serve as the converter cold charge, traditional converter cold charge is replaced, meanwhile, iron, cobalt, nickel and zinc elements in the converter cold charge are efficiently recycled, and the purposes of reducing cost and improving efficiency are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of chemical metallurgy, and more specifically, to a method for comprehensive utilization of sulfuric acid slag. Background Art

[0002] Sulfuric acid slag is the byproduct of slag produced when pyrite is used to prepare sulfuric acid. Valuable elements in it include iron, zinc, cobalt, nickel, etc. With the development of my country's sulfuric acid industry, sulphuric acid slag has become a major source of environmental pollution. The comprehensive utilization of sulphuric acid slag can not only reduce environmental pollution, but also improve resource utilization efficiency and have significant economic benefits. The comprehensive utilization of sulphuric acid slag is a multi-faceted and multi-technical comprehensive process. It is necessary to select appropriate treatment methods and processes according to specific circumstances to achieve the goal of maximizing resource utilization and environmental protection. Although the comprehensive utilization of sulphuric acid slag has made some progress, it still faces some challenges.

[0003] At present, the technologies and processes for comprehensive utilization of sulfuric acid slag mainly include the following:

[0004] (1) Chemical treatment: Using aqua regia as a leaching agent can effectively remove sulfur from sulfate slag and enrich iron. This process involves the dissolution of CaSO4, the oxidative dissolution of metal sulfides, and the dissolution of alkaline oxides. By adjusting the dosage of reagents, leaching temperature and time, the iron recovery rate and sulfur content can be optimized.

[0005] (2) Chemical-magnetic separation combined method: This method uses chemical leaching to remove sulfur, and then combines it with magnetic separation technology to enrich iron. It can not only improve the iron grade, but also reduce the sulfur grade, making the sulfate slag more suitable for the production of iron concentrate or iron oxide red pigment and other products.

[0006] (3) Coal-based reduction smelting method: By mixing sulfuric acid slag with bituminous coal and performing reduction smelting under certain basicity, roasting temperature and time conditions, pearl iron with high iron recovery rate can be obtained. In addition, due to the high sulfur content of the obtained pearl iron, it is also suitable for smelting sulfur-based free-cutting steel.

[0007] (4) Rotary kiln roasting method: Using a rotary kiln to roast sulfuric acid slag can effectively reduce Fe2O3 in it, and improve the iron recovery rate through ball milling and magnetic separation processes. This method can achieve a desulfurization rate of more than 85% under certain conditions (inclination angle 0.8°, rotation speed 12r / min).

[0008] (5) Coarse particle tailings discarding - grinding - magnetic separation - flotation desulfurization method: This comprehensive process uses sulfuric acid slag to obtain iron ore concentrate with higher iron content and lower sulfur content. The iron recovery rate is 51.30% and the sulfur content is 0.22%.

[0009] (6) Screening-rinsing-fine grinding-selective flocculation-reverse flotation process: This method determines the appropriate process flow by analyzing the mineralogical properties of the sulfate slag, and can obtain iron concentrate with a total iron content of 65.34%, a sulfur content of 0.037%, and a silicon content of 5.54%.

[0010] (7) Improve the balling performance as a pelletizing raw material: After grinding the sulfate slag, its particle size and balling performance are significantly improved. At a specific particle size level and bentonite addition ratio, the balling performance of the sulfate slag is good and can be used as a pelletizing raw material to prepare pellets.

[0011] In summary, from the above existing technology and process description, it can be seen that the existing technologies and processes for comprehensive utilization of sulfuric acid slag require pyrometallurgy, magnetic separation or chemical leaching to effectively separate and recover the Fe element therein. The process is relatively long, and it needs to be put into the ironmaking process in the next step to realize the reuse of iron. As a raw material for the pelletizing process, the seventh method has the problem of sulfur emission, and it is necessary to build a corresponding desulfurization process for use, which increases the investment cost.

[0012] At present, the steel industry is facing the challenge of sustainable development of iron ore resources, and the competition is very fierce. Steel enterprises have been committed to reducing costs and increasing efficiency in production, and the use of reasonable technology and processes to efficiently use various cost-effective iron-containing resources has always been the pursuit of steel enterprises. As a cheap iron-containing resource, sulfuric acid slag has a good cost-effectiveness. Therefore, it is necessary to provide a new method for the comprehensive utilization of sulfuric acid slag to help steel enterprises achieve the purpose of reasonable and efficient use of sulfuric acid slag. Summary of the invention

[0013] The present application provides a method for the comprehensive utilization of sulfuric acid slag, which utilizes the process characteristics of the converter itself to press the sulfuric acid slag into briquettes as converter cold material, replacing the traditional converter cold material, and at the same time efficiently recovering and utilizing the iron, cobalt, nickel and zinc elements therein, thereby achieving the purpose of reducing costs and increasing efficiency.

[0014] The present application provides a method for comprehensive utilization of sulfuric acid slag, which adopts the following technical scheme:

[0015] A method for comprehensive utilization of sulfuric acid slag, the method specifically comprising the following steps:

[0016] Grinding the sulfuric acid slag and matching the particle sizes, adding water and a binder to the matched materials and pressing them into agglomerates to form dry agglomerates; sending the dry agglomerates into a converter for use as cold materials;

[0017] The particle size matching method is as follows: materials with a particle size of 0.3 mm < ≤ 0.5 mm account for 10-20%; materials with a particle size of 0.045 mm < ≤ 0.3 mm account for 20-40%; materials with a particle size of ≤ 0.045 mm account for 40-70%;

[0018] Add the water so that the moisture content of the prepared materials is 7.5-8.0%;

[0019] The added amount of the binder accounts for 3-5% of the weight percentage of the prepared materials.

[0020] Optionally, the particle size is matched as follows: materials with a particle size of 0.3 mm < ≤ 0.5 mm account for 15-20%; materials with a particle size of 0.045 mm < ≤ 0.3 mm account for 20-30%; and materials with a particle size of ≤ 0.045 mm account for 50-65%.

[0021] Optionally, the strength of the dry mass is not less than 800N.

[0022] Optionally, the ball milling time is 3-5 min.

[0023] Optionally, the iron oxide, cobalt oxide or iron, cobalt and nickel in cobalt ferrite and nickel-iron oxide in the sulfate slag can be used as alloy raw materials required for molten steel refining after being reduced to a metallic state.

[0024] Optionally, the zinc element in the sulfuric acid slag escapes in the form of steam and is recovered by cooling and condensing or adhering to dust particles.

[0025] In summary, this application has the following beneficial effects:

[0026] In the present application, the sulfuric acid slag is ground and matched according to a reasonable particle size distribution, and then a proper amount of water and a binder are added, and the slag is pressed into agglomerates by a roller press. The obtained agglomerates can be dried or air-dried according to actual production conditions to obtain dry agglomerates, so as to achieve the strength required for converter cold material. The dry agglomerates are then sent to the converter as cold material.

[0027] Iron oxides, cobalt oxides or cobalt ferrite, nickel iron oxides, etc. in the sulfate slag are reduced by carbon in the molten iron and enter the molten iron. These elements can be used as alloy raw materials for later molten steel refining. The zinc element mainly exists in the form of ZnFe2O4, which is reduced to Zn metal by carbon in the molten iron and escapes in the form of Zn vapor. After entering the flue, it is oxidized into zinc oxide or zinc secondary oxide, and is recovered by cooling and condensing in the flue or adhering to dust particles.

[0028] This application utilizes the process characteristics of the converter itself to press the sulfuric acid slag into agglomerates as converter cold materials. In the traditional converter process, sintered ore, pelletized ore, scrap steel, etc. are usually used as cold materials for steelmaking, and the price is about 1,000 yuan per ton. After adopting the technical solution of this application, the total cost of sulfuric acid slag agglomerates is about 500 yuan / ton. Using sulfuric acid slag agglomerates as cold materials can reduce the cost of the steelmaking process. At the same time, the technical solution of this application can efficiently recycle the iron, cobalt, nickel, and zinc elements therein, which solves the pollution problem of sulfuric acid slag to the environment on the one hand, and helps steel mills achieve the purpose of reducing costs and increasing efficiency on the other hand. DETAILED DESCRIPTION

[0029] Before describing the embodiments of the present application in detail, it should be understood that the terms used herein are only used for the purpose of describing specific embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by ordinary technicians in the field to which the terms belong.

[0030] The present application provides a method for comprehensive utilization of sulfuric acid slag, which specifically comprises the following steps:

[0031] (1) Grind the sulfuric acid slag for 3-5 minutes and perform particle size matching. The particle size matching method is as follows: 10-20% of the material has a particle size of 0.3 mm < ≤ 0.5 mm; 20-40% of the material has a particle size of 0.045 mm < ≤ 0.3 mm; and 40-70% of the material has a particle size of ≤ 0.045 mm.

[0032] (2) adding water to the prepared materials until the moisture content of the prepared materials is 7.5-8.0%, and adding a binder accounting for 3-5% by weight of the prepared materials to mix well, and then pressing the lumps, and forming dry lumps by drying or air-drying, so that the strength of the dry lumps is not less than 800N.

[0033] (3) The obtained dry mass is sent to a converter for use as cold material.

[0034] This application utilizes the process characteristics of the converter itself to press the sulfuric acid slag into agglomerates as converter cold materials. In the traditional converter process, sintered ore, pelletized ore, scrap steel, etc. are usually used as cold materials for steelmaking, and the price is about 1,000 yuan per ton. After adopting the technical solution of this application, the total cost of sulfuric acid slag agglomerates is about 500 yuan / ton. Using sulfuric acid slag agglomerates as cold materials can reduce the cost of the steelmaking process. At the same time, the technical solution of this application can efficiently recycle the iron, cobalt, nickel, and zinc elements therein, which solves the pollution problem of sulfuric acid slag to the environment on the one hand, and helps steel mills achieve the purpose of reducing costs and increasing efficiency on the other hand.

[0035] To make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application are described clearly and completely below. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0036] The present application is further described in detail below in conjunction with the embodiments and performance test results.

[0037] In the following examples, binder A was purchased from Gongyi Jinao Refractory Materials Co., Ltd., model number CBS; binder B was purchased from Gongyi Jinao Refractory Materials Co., Ltd., model number CBS-D.

[0038] Example

[0039] Example 1

[0040] This embodiment provides a method for comprehensive utilization of sulfuric acid slag.

[0041] The specific steps include:

[0042] (1) Grind the sulfuric acid slag with a ball mill for 3 minutes and perform particle size matching. The particle size matching is as follows: 10% of the material has a particle size of 0.3 mm < ≤ 0.5 mm; 20% of the material has a particle size of 0.045 mm < ≤ 0.3 mm; and 70% of the material has a particle size of ≤ 0.045 mm.

[0043] (2) Water was added to the prepared materials until the moisture content of the prepared materials was 7.5%, and a binder A accounting for 3% by weight of the prepared materials was added and mixed. The mixture was then pressed into lumps using a double-roll ball press and dried for 48 hours. The dry lump strength was 867N.

[0044] (3) The obtained dry mass is sent to a converter for use as cold material.

[0045] Example 2-16

[0046] Embodiments 2-16 respectively provide a method for comprehensive utilization of sulfuric acid slag. The difference between the above embodiment and embodiment 1 is that the parameters involved in the method are different, as shown in Table 1, and the rest are consistent with embodiment 1.

[0047] The differences between Examples 1-16 are as follows:

[0048] The difference between Examples 1-5 is that: while keeping the weight percentage of the material with "0.045mm<particle size≤0.3mm" unchanged, the weight percentage of the material with "0.3mm<particle size≤0.5mm" is adjusted, and the weight percentage of the material with "particle size≤0.045mm" is adaptively adjusted.

[0049] The difference between Example 6-9 and Example 3 is that: while keeping the weight percentage of the material with "0.3mm<particle size≤0.5mm" unchanged, the weight percentage of the material with "0.045mm<particle size≤0.3mm" is adjusted, and the weight percentage of the material with "particle size≤0.045mm" is adaptively adjusted.

[0050] The difference between Example 10-11 and Example 7 is that: while keeping the weight percentage of the material with "particle size ≤ 0.045mm" unchanged, the weight percentage of the material with "0.045mm<particle size ≤ 0.3mm" is adjusted, and the weight percentage of the material with "0.3mm<particle size ≤ 0.5mm" is adaptively adjusted.

[0051] The difference between Example 12 and Example 7 is that the type of adhesive is different.

[0052] The difference between Examples 13-15 and Example 12 is that the weight percentage of the binder is different.

[0053] The difference between Example 16 and Example 12 is that the drying time of the dried lumps is different.

[0054] Table 1 Parameters involved in the method provided in the embodiment

[0055]

[0056] Comparative Example

[0057] Comparative Examples 1-8

[0058] Comparative Examples 1-8 respectively provide a method for comprehensive utilization of sulfuric acid slag. The difference between the above comparative examples and Example 1 is that the parameters involved in the method are different, as shown in Table 1, and the rest are consistent with Example 1.

[0059] The differences between Comparative Examples 1-8 are as follows:

[0060] The difference between Comparative Example 1-2 and Example 1 is that: while keeping the weight percentage of the material with "0.045mm<particle size≤0.3mm" unchanged, the weight percentage of the material with "0.3mm<particle size≤0.5mm" is adjusted, and the weight percentage of the material with "particle size≤0.045mm" is adaptively adjusted.

[0061] The difference between Comparative Example 3-4 and Example 3 is that: while keeping the weight percentage of the material with "0.3mm<particle size≤0.5mm" unchanged, the weight percentage of the material with "0.045mm<particle size≤0.3mm" is adjusted, and the weight percentage of the material with "particle size≤0.045mm" is adaptively adjusted.

[0062] The difference between Comparative Examples 5-6 and Example 7 is that the weight percentage of the binder is different.

[0063] The difference between Comparative Example 7-8 and Example 7 is that the moisture content of the materials is different after adding water.

[0064] Performance testing

[0065] The strength of the dry lumps prepared in the above examples was tested respectively. The test results are shown in Table 1.

[0066] Compressive strength testing method: It is measured using a digital display compressive strength testing machine, and the average compressive strength of ten test blocks is taken as the compressive strength of the test block.

[0067] According to the test results in Table 1, when the particle size is matched in the following manner: 10-20% of the material is 0.3mm<particle size≤0.5mm; 20-40% of the material is 0.045mm<particle size≤0.3mm; 40-70% of the material is ≤0.045mm, the strength of the obtained dry agglomerates is greater than 800N, which can meet the strength requirements of agglomerates for cold materials. In the particle size matching composition, coarse or very fine particles or too high a proportion of intermediate particles are not conducive to the strength of the dry agglomerates. Furthermore, when the particle size is matched in the following manner: 15-20% of the material is 0.3mm<particle size≤0.5mm; 20-30% of the material is 0.045mm<particle size≤0.3mm; 50-65% of the material is ≤0.045mm, the strength of the obtained dry agglomerates is greater than 1000N. In particular, the most suitable particle size composition ratio is 0.3mm<particle size ≤0.5mm:0.045mm<particle size ≤0.3mm:particle size ≤0.045mm, which is 15:30:55.

[0068] In addition, as the amount of binder increases, the strength of the dry mass gradually increases, but considering the cost of the binder, the amount of binder is usually selected to be 3-5%. At the same time, it can be seen that the appropriate moisture content of the mixture is 7.5-8.0%. If the moisture content of the mixture is too low, the briquetting is not used, and the strength of the dry mass obtained is only about 500N. If the moisture content of the mixture is too high, the roller sticking phenomenon will occur during the production process, resulting in the inability to proceed smoothly.

[0069] The technical solution of the present application utilizes the process characteristics of the converter itself to press the sulfuric acid slag into briquettes as converter cold material, replacing the traditional converter cold material, while efficiently recycling the iron, cobalt, nickel and zinc elements therein, thereby achieving the purpose of reducing costs and increasing efficiency.

[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for comprehensive utilization of sulfuric acid slag, characterized in that: The method specifically comprises the following steps: Grinding the sulfuric acid slag and matching the particle sizes, adding water and a binder to the matched materials and pressing them into agglomerates to form dry agglomerates; sending the dry agglomerates into a converter for use as cold materials; The particle size matching method is: 10-20% of the materials with a particle size of 0.3mm < ≤ 0.5mm; 20-40% of the materials with a particle size of 0.045mm < ≤ 0.3mm; 40-70% of the materials with a particle size of ≤ 0.045mm; Add the water so that the moisture content of the prepared materials is 7.5-8.0%; The added amount of the binder accounts for 3-5% by weight of the matched materials.

2. The method for comprehensive utilization of sulphuric acid slag according to claim 1, characterized in that: The particle size matching method is: materials with a particle size of 0.3mm < ≤ 0.5mm account for 15-20%; materials with a particle size of 0.045mm < ≤ 0.3mm account for 20-30%; materials with a particle size of ≤ 0.045mm account for 50-65%.

3. The method for comprehensive utilization of sulphuric acid slag according to claim 1, characterized in that: The strength of the dry mass is not less than 800N.

4. The method for comprehensive utilization of sulphuric acid slag according to claim 1, characterized in that: The ball milling time is 3-5 min.

5. The method for comprehensive utilization of sulphuric acid slag according to claim 1, characterized in that: The iron, cobalt and nickel in the iron oxide, cobalt oxide or cobalt ferrite and nickel-iron oxide in the sulfate slag can be used as alloy raw materials required for molten steel refining after being reduced to a metallic state.

6. The method for comprehensive utilization of sulphuric acid slag according to claim 1, characterized in that: The zinc element in the sulfuric acid slag escapes in the form of steam and is recovered by cooling and condensing or adhering to dust particles.