Slag bath dynamic balance method in electroslag smelting process
By calculating the mass ratio of each component in real time based on temperature during the electroslag smelting process, using different brands of small-particle pre-melted slag to form low-melting-point eutectic compounds, and dynamically adjusting the composition of the slag pool, the problem of unstable slag liquid composition is solved and achieved This ensures the controllability and quality stability of the smelting process.
Patent Information
- Application Number
- CN202410731498.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the electroslag smelting process, the composition of the slag liquid is unstable, resulting in fluctuations in the smelting process. The existing slag filling process cannot effectively maintain the balance of the slag pool components, especially the decrease in the content of CaF2 and Al2O3 and the increase in the content of CaO, resulting in slag blockage, slag Changes in properties and slag temperature, and the existing simulation methods are inconsistent with the actual reaction, resulting in obvious composition fluctuations.
Different brands of small-particle pre-melted slag are added at different smelting stages. The mass ratio of each component is calculated in real time based on the temperature at the interface between the slag pool and the ingot. The quantity and composition of the replenished slag are optimized through artificial intelligence algorithms to form a low melting point cobalt. Crystal compound, dynamically adjust the composition of the slag pool to ensure the dynamic balance of the slag pool.
By dynamically adjusting the composition of the slag pool, drastic fluctuations when adding fluorite powder and alumina powder separately are avoided, the stability of the composition of the slag pool and the improvement of the smelting effect are achieved, and the controllability and quality stability of the smelting process are ensured.
Smart Images

Figure CN118773446A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electroslag smelting, and in particular relates to a slag pool dynamic balancing method in the electroslag smelting process. Background Art
[0002] Electroslag metallurgy is a fire refining method that uses electric current to pass through electroslag as a resistor to convert electrical energy into heat energy to melt metals or alloys. Its basic principle is to melt and purify metal droplets through a slag pool. In this process, ensuring the stability of the slag pool thickness, composition, and physical properties is the key to ensuring stable metallurgical quality. However, in the actual production process, slag skin will continue to form on the surface of the electroslag ingot, resulting in continuous loss of slag liquid, and the thickness of the slag pool is getting shallower and shallower. At the end of smelting, the remaining slag liquid is even less than 70% of the initial slag liquid, which will obviously cause significant fluctuations in the smelting process.
[0003] To deal with this situation, the method of supplementing slag during the smelting process is usually adopted, and the loss caused by the slag skin is compensated by adding slag of the same composition. However, this method can only maintain the stability of the slag amount, but cannot maintain the stability of the slag liquid composition. Because the composition of the lost slag skin is not consistent with the composition of the slag pool, this is caused by the separation and crystallization during the solidification of the slag liquid. The slag skin will be significantly enriched with CaF2 and Al2O3, resulting in a significant decrease in the content of CaF2 and Al2O3 in the remaining slag pool, while the CaO content continues to increase, which leads to significant changes in slag resistance, slag properties, and slag temperature. This change cannot be compensated by the slag supplementation process with the original composition slag.
[0004] At present, the existing technology can also supplement the content of CaF2 and Al2O3 in the slag pool by adding fluorite powder and alumina powder in different proportions separately. This method is an improvement over the traditional original component slag supplement process, but the melting points of fluorite powder and alumina powder are very different, and the melting point of alumina powder is significantly higher than that of the slag pool, which will cause the slag pool to fluctuate violently during the slag addition process, which in turn leads to increased risks of segregation and slag inclusion. Patent application CN202310380594.2 discloses a slag pool dynamic balance technology, but it obtains the participation amount of each component in the electroslag metallurgical process through ideal model simulation. This simulation method is not completely consistent with the physical and chemical reactions in the actual crystallizer, resulting in the calculated results being inconsistent with the actual situation, and the slag pool composition fluctuations are still very obvious.
[0005] There is currently no more advanced way to effectively resolve this contradiction. Summary of the invention
[0006] The purpose of the present invention is to solve the problems existing in the above-mentioned prior art and to provide a process for adding slag of different grades in stages. In different smelting stages during the smelting process, small particles of pre-melted slag with different components and quantities are added to dynamically compensate for the changes in the slag amount and slag composition in the slag pool.
[0007] The present invention provides a slag pool dynamic balancing method, comprising the following steps:
[0008] S1. Initial slag selection
[0009] 100 kg of 622 pre-melted slag with a particle size of 7-10 mm is selected, and the slag composition is 60% CaF2, 20% Al2O3, and 20% CaO by mass ratio. After baking, it is put into the slag feeder and added at the beginning of smelting;
[0010] S2. Selection of supplementary slag
[0011] 6kg of 622-01 pre-melted slag, 5.5kg of 622-02 pre-melted slag, 5kg of 622-03 pre-melted slag, 4.5kg of 622-04 pre-melted slag and 4kg of 622-05 pre-melted slag with a particle size of 2 to 4mm are selected and put in a baking furnace for use; wherein, the mass proportions of CaF2, Al2O3 and CaO phases in the 622-01 to 622-05 pre-melted slags all change in a gradient manner, and the 622-05 pre-melted slag does not contain CaO;
[0012] S3. Add the initial slag to the crystallizer, start smelting, obtain the temperature T at the interface between the slag pool and the ingot, calculate the components involved in the interface reaction at the current temperature T, and the calculation model is as follows:
[0013] All chemical reactions at the interface reach equilibrium, and the equilibrium state is expressed as formula (1):
[0014]
[0015] Where ΔG represents the change in Gibbs free energy, R represents the gas constant and R=8.314 J / (mol·K), the unit of temperature T is K, a represents the activity of the component, r represents the activity coefficient of the component in the slag pool, X represents the molar fraction of the component in the slag pool, f represents the activity coefficient of a component in the ingot, [pctM] and [pctO] represent the mass percentages of M and O in the ingot, respectively, where M and O represent an element in the slag pool and the ingot, respectively, and the two can react chemically to generate MO n , * indicates the interface;
[0016] At the interface, the concentration gradient is the driving force for the diffusion of each component. The diffusion mass transfer flux density at the interface is calculated using formula (2) (3):
[0017]
[0018] Among them, J M and Indicates M and MO n The molar mass transfer flux density, kM and are the mass transfer coefficients of each component, ρ represents the density, M M and represent molecular weight, b represents the bulk region, * represents the interface, [pctM] and [pctMO n ] represent mass percentages respectively;
[0019] When the interface is in a stable state, it is assumed that and the number of anions is equal to the number of cations;
[0020] Combining formulas (1)-(3), the mass ratio of each component at the interface is calculated;
[0021] S4. At preset time intervals, according to the mass ratio of each component at the interface obtained in step S3, compare it with the initial slag composition, and based on the comparison result, select one or more pre-melted slags from 622-01 to 622-05, put them into the slag feeder after proportioning, and put them into the crystallizer by the slag feeder to maintain the dynamic balance of the slag pool.
[0022] Furthermore, the composition of the 622-05 pre-melted slag is 73% CaF2 and 27% Al2O3 by mass, and does not contain CaO; the composition of the 622-01 pre-melted slag is the same as the initial slag.
[0023] Furthermore, in step S4, the preset time is determined according to the composition change curve at the interface, or the preset time is determined by dividing the total time required for smelting by an average.
[0024] Furthermore, the slag pool dynamic balancing method according to claim 1 is characterized in that: in the pre-melted slag, each component forms a low melting point eutectic compound.
[0025] Furthermore, the number of times the pre-molten slag is added during the smelting process is greater than or equal to 3;
[0026] Furthermore, in step S4, a linear regression method, a random forest method or a decision tree method is used to optimize the comparison result.
[0027] In the traditional electroslag production process, only one brand of slag will be used for one furnace of smelting. Compared with the prior art, the present invention adds small-particle pre-melted slag with different components and quantities at different smelting stages in the smelting process to dynamically compensate for the changes in the amount of slag and slag composition in the slag pool. In the pre-melted slag, each component forms a low-melting point eutectic compound, so it will melt quickly and stably after being added to the slag pool, and will not cause drastic fluctuations when fluorite powder and alumina powder are added separately, effectively solving this long-standing process contradiction. The mass ratio of each component is calculated in real time based on the temperature at the interface between the slag pool and the ingot, and an artificial intelligence algorithm is used to optimize the amount of slag replenishment, making the slag replenishment process more accurate and controllable, which is beneficial to maintaining the dynamic balance of the slag pool and improving the smelting effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the electroslag smelting principle.
[0029] Figure 2 Flow chart of the slag pool dynamic balancing method provided by the present invention. DETAILED DESCRIPTION
[0030] Figure 1 It is a schematic diagram of the principle of electroslag smelting. The basic smelting process is to add slag to the water-cooled crystallizer 1, insert one end of the electrode 5 into the slag pool 2 in the crystallizer and energize it. The electrode 5, the slag pool 2 and the ingot 4 are connected to the external power supply to form a power supply circuit. After power is turned on, the electrode 5 and the slag with resistance value generate resistance heat, and the slag and the electrode heat up rapidly. After reaching a certain temperature, the electrode begins to melt, and its end melts and gathers into small metal droplets 6. As the smelting progresses, the volume of the small droplets gradually increases, and they fall away from the end of the electrode 5, pass through the slag pool 2 and enter the bottom to form a metal molten pool 3. Under the cooling effect of the water-cooled crystallizer, the liquid metal gradually solidifies from bottom to top into an ingot 4.
[0031] During the smelting process, the composition of the slag pool changes as the metal continues to solidify. The present invention proposes a slag pool dynamic balance method, comprising the following steps:
[0032] S1. Initial slag selection
[0033] 100 kg of 622 pre-melted slag with a particle size of 7-10 mm is selected, and the slag composition is 60% CaF2, 20% Al2O3, and 20% CaO by mass ratio. After baking, it is put into the slag feeder and added at the beginning of smelting;
[0034] S2. Selection of supplementary slag
[0035] 6kg of 622-01 pre-melted slag, 5.5kg of 622-02 pre-melted slag, 5kg of 622-03 pre-melted slag, 4.5kg of 622-04 pre-melted slag and 4kg of 622-05 pre-melted slag with a particle size of 2 to 4mm are selected and put in a baking furnace for use; wherein, the mass proportions of CaF2, Al2O3 and CaO phases in the 622-01 to 622-05 pre-melted slags all change in a gradient manner, and the 622-05 pre-melted slag does not contain CaO;
[0036] S3. Add the initial slag to the crystallizer, start smelting, obtain the temperature T at the interface between the slag pool and the ingot, calculate the components involved in the interface reaction at the current temperature T, and the calculation model is as follows:
[0037] All chemical reactions at the interface reach equilibrium, and the equilibrium state is expressed as formula (1):
[0038]
[0039] Where ΔG represents the change in Gibbs free energy, R represents the gas constant and R=8.314 J / (mol·K), the unit of temperature T is K, a represents the activity of the component, r represents the activity coefficient of the component in the slag pool, X represents the molar fraction of the component in the slag pool, f represents the activity coefficient of a component in the ingot, [pctM] and [pctO] represent the mass percentages of M and O in the ingot, respectively, where M and O represent an element in the slag pool and the ingot, respectively, and the two can react chemically to generate MO n , * indicates the interface;
[0040] At the interface, the concentration gradient is the driving force for the diffusion of each component. The diffusion mass transfer flux density at the interface is calculated using formula (2) (3):
[0041]
[0042] Among them, J M and Indicates M and MO n The molar mass transfer flux density, k M and are the mass transfer coefficients of each component, ρ represents the density, M M and represent molecular weight, b represents the bulk region, * represents the interface, [pctM] and [pctMO n ] represent mass percentages respectively;
[0043] When the interface is in a stable state, it is assumed that and the number of anions is equal to the number of cations;
[0044] Combining formulas (1)-(3), the mass ratio of each component at the interface is calculated;
[0045] S4. At preset time intervals, according to the mass ratio of each component at the interface obtained in step S3, compare it with the initial slag composition, and based on the comparison result, select one or more pre-melted slags from 622-01 to 622-05, put them into the slag feeder after proportioning, and put them into the crystallizer by the slag feeder to maintain the dynamic balance of the slag pool.
[0046] Furthermore, the composition of the 622-05 pre-melted slag is 73% CaF2 and 27% Al2O3 by mass, and does not contain CaO; the composition of the 622-01 pre-melted slag is the same as the initial slag.
[0047] Furthermore, in step S4, the preset time is determined according to the composition change curve in the slag pool, or the preset time is determined by dividing the total time required for smelting by an average.
[0048] Furthermore, the slag pool dynamic balancing method according to claim 1 is characterized in that: in the pre-melted slag, each component forms a low melting point eutectic compound.
[0049] Furthermore, the number of times the pre-slag is added during the smelting process is greater than or equal to 3.
[0050] Furthermore, in step S4, a linear regression method, a random forest method or a decision tree method is used to optimize the comparison result.
[0051] In the traditional electroslag production process, only one brand of slag will be used for one furnace of smelting. Compared with the prior art, the present invention adds small-particle pre-melted slag with different components and quantities at different smelting stages in the smelting process to dynamically compensate for the changes in the amount of slag and slag composition in the slag pool. In the pre-melted slag, each component forms a low-melting point eutectic compound, so it will melt quickly and stably after being added to the slag pool, and will not cause drastic fluctuations when fluorite powder and alumina powder are added separately, effectively solving this long-standing process contradiction. The mass ratio of each component is calculated in real time based on the temperature at the interface between the slag pool and the ingot, and an artificial intelligence algorithm is used to optimize the amount of slag replenishment, making the slag replenishment process more accurate and controllable, which is beneficial to maintaining the dynamic balance of the slag pool and improving the smelting effect.
[0052] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0053] In the description of the present invention, unless otherwise specified, the terms "upper", "lower", "left", "right", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.
[0054] Finally, it should be explained that the above technical solution is only one implementation method of the present invention. For those skilled in the art, it is easy to make various types of improvements or modifications based on the application methods and principles disclosed in the present invention, and it is not limited to the method described in the above specific implementation method of the present invention. Therefore, the method described above is only preferred and does not have a restrictive meaning.
Claims
1. A method for dynamically balancing a slag pool during electroslag smelting, comprising the following steps: S1. Initial slag selection 100 kg of 622 pre-melted slag with a particle size of 7-10 mm is selected, and the slag composition is 60% CaF2, 20% Al2O3, and 20% CaO by mass ratio. After baking, it is put into the slag feeder and added at the beginning of smelting; S2. Selection of supplementary slag 6kg of 622-01 pre-melted slag, 5.5kg of 622-02 pre-melted slag, 5kg of 622-03 pre-melted slag, 4.5kg of 622-04 pre-melted slag and 4kg of 622-05 pre-melted slag with a particle size of 2 to 4mm are selected and put in a baking furnace for use; wherein, the mass proportions of CaF2, Al2O3 and CaO phases in the 622-01 to 622-05 pre-melted slags all change in a gradient manner, and the 622-05 pre-melted slag does not contain CaO; S3. Add the initial slag to the crystallizer, start smelting, obtain the temperature T at the interface between the slag pool and the ingot, calculate the components involved in the interface reaction at the current temperature T, and the calculation model is as follows: At the interface, all chemical reactions reach equilibrium, and the equilibrium state is expressed as formula (1): Where ΔG represents the change in Gibbs free energy, R represents the gas constant and R=8.314 J / (mol·K), the unit of temperature T is K, a represents the activity of the component, r represents the activity coefficient of the component in the slag pool, X represents the molar fraction of the component in the slag pool, f represents the activity coefficient of a component in the ingot, [pctM] and [pctO] represent the mass percentages of M and O in the ingot, respectively, where M and O represent an element in the slag pool and the ingot, respectively, and the two can react chemically to generate MO n , * indicates the interface; At the interface, the concentration gradient is the driving force for the diffusion of each component. The diffusion mass transfer flux density at the interface is calculated using formula (2) (3): Among them, J M and Indicates M and MO n Molar mass transfer flux density of the component, k M and are the mass transfer coefficients of each component, ρ represents the density, M M and represent molecular weight, b represents the bulk region, * represents the interface, [pctM] and [pctMO n ] represent mass percentages respectively; When the interface is in a stable state, it is assumed that and the number of anions is equal to the number of cations; Combining formulas (1)-(3), the mass ratio of each component at the interface is calculated; S4. At preset time intervals, the contents of CaF2, Al2O3 and CaO in the slag pool obtained in step S3 are compared with the initial slag composition. Based on the comparison results, one or more pre-melted slags are selected from 622-01 to 622-05, and the pre-melted slags are placed in a slag feeder after proportioning. The slag feeder then feeds the pre-melted slags into the crystallizer to maintain the dynamic balance of the slag pool.
2. The slag pool dynamic balancing method according to claim 1, characterized in that: The composition of the 622-05 pre-melted slag is 73% CaF2 and 27% Al2O3 by mass ratio, and does not contain CaO; the composition of the 622-01 pre-melted slag is the same as the initial slag.
3. The slag pool dynamic balancing method according to claim 1, characterized in that: In step S4, the preset time is determined according to the composition change curve in the slag pool, or the preset time is determined by evenly dividing the total time required for smelting.
4. The slag pool dynamic balancing method according to claim 1, characterized in that: In the pre-melted slag, each component forms a low melting point eutectic compound.
5. The slag pool dynamic balancing method according to claim 1, characterized in that: The number of times the pre-slag is added during the smelting process is greater than or equal to 3.
6. The slag pool dynamic balancing method according to claim 1, characterized in that: In step S4, a linear regression method, a random forest method or a decision tree method is used to optimize the comparison result.
Citation Information
Patent Citations
Ti element control method for Ti-contained corrosion resistant alloy ingot extracting electroslag remelting slab
CN104212977A
Method for predicting element burning loss and adjusting slag system based on molecular ion coexistence theory
CN114990345A
Slag bath dynamic balance method in electroslag smelting process
CN116607015A
Electroslag refining process
GB1338061A
Cited By
Rapid batching method for preparing titanium alloy electrode through VAR smelting
CN119943177A