Method for simultaneously extracting lithium and aluminum from clay type lithium ore
Through pressurized alkali leaching and subsequent adsorption, desorption, and carbon separation processes, the problem of difficulty in extracting lithium and aluminum from clay-type lithium ores is solved, efficient comprehensive utilization of lithium and aluminum resources is achieved, and energy consumption and production costs are reduced.
Patent Information
- Application Number
- CN202410793577.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to effectively extract lithium and aluminum from clay-type lithium ores simultaneously with existing technology, and there are problems such as high energy consumption, high production costs, and low lithium leaching rate.
The pressurized alkali leaching method is used to destroy the structure of clay-type lithium ore, and the adsorption, desorption and carbon separation processes are combined to obtain lithium-rich solution and aluminum hydroxide products respectively, avoiding the high-temperature roasting process, simplifying the process and reducing energy consumption.
The comprehensive utilization of lithium and aluminum in clay-type lithium ores has been achieved. The lithium leaching rate is as high as more than 89.31%, and the aluminum leaching rate is as high as more than 85.1%. The comprehensive recovery rate is significantly improved, with low production energy consumption and less waste residue.
Smart Images

Figure CN118773453A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for simultaneously extracting lithium and aluminum from clay-type lithium ore. Background Art
[0002] With the growing demand for clean energy and sustainable development, lithium batteries play a key role in energy transformation, transportation and energy storage systems. The demand for lithium salts has surged, and traditional lithium mineral resources cannot meet the supply of lithium. There is an urgent need to develop and utilize new lithium mineral resources. Due to the large reserves of clay-type lithium ore, if it can be developed using appropriate methods, it will be a very promising source of lithium demand.
[0003] At present, clay-type lithium ores can be divided into volcanic type, carbonate type and Jadar type according to the causes of mineralization. Large-scale clay-type lithium ores have been discovered in the central Yunnan region, which are carbonate clay-type lithium ores associated with bauxite. Lithium mainly exists in the form of minerals or isomorphously wrapped or intermixed in clay-type lithium ores, which are difficult to release and difficult to mine. Most of them are processed by processes such as "roasting-sulfuric acid leaching" and "composite additive roasting-leaching", which have obvious disadvantages. For example, the roasting temperature is as high as 400°C, which consumes a lot of heat energy. Roasting aids need to be added during the roasting process. The equipment requirements are relatively high. In addition, elements such as S in the ore will volatilize during roasting to pollute the environment, and additional equipment is required to treat the exhaust gas, resulting in increased production costs.
[0004] CN116240399A discloses a method for selectively leaching lithium from clay-type lithium ore, which comprises roasting and activating the clay-type lithium ore at a high temperature of 500-600°C, and then using fluoride salt as a leaching agent to leach lithium under weak alkaline conditions, with a lithium leaching rate of 85.13%. The lithium leaching rate of this method is relatively low, and there is still much room for improvement; the roasting process has a high temperature and consumes a lot of energy; and the simultaneous recovery and utilization of aluminum resources in the clay-type lithium ore is not achieved.
[0005] CN111575504A discloses a method for efficiently leaching lithium from lithium-containing clay rock, the main steps of which are firstly crushing the raw ore to less than 2 mm, then mixing with concentrated sulfuric acid for slurry preparation, heat treating and maturing at 150-210°C for 1-4 hours, and then leaching the clinker at 80°C; this method will introduce a large amount of impurities into the leachate, including iron, magnesium, calcium, potassium, sodium, etc., and there will also be a large amount of residual acid solution. The high concentration of inorganic acid not only increases the corrosiveness to the leaching equipment, but also introduces acid impurities into the subsequent deacidification and purification process, requiring a large amount of alkali to neutralize the excess acid and produce a large amount of neutralization slag, and also fails to simultaneously recycle the aluminum resources in the clay-type lithium ore.
[0006] At present, most of the research has only done the lithium leaching process, but has not conducted in-depth research on the subsequent lithium leaching solution removal. The impurity content in the leaching solution of the acid lithium extraction process is relatively high, especially for clay-type lithium ore. Due to the low lithium content and high aluminum content, lithium is easily lost by co-precipitation with aluminum hydroxide in the traditional impurity removal process, which is not conducive to the comprehensive recovery of resources; and the traditional precipitation method of impurity removal requires the addition of a large amount of alkali material. For low-grade clay-type lithium ores, the process production cost is too high; it can be seen that there is currently a lack of a short-process, low-energy method for simultaneously extracting lithium and aluminum from clay-type lithium ores.
[0007] Therefore, it is urgent to develop a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is of great significance to ensuring the supply of lithium and aluminum resources. Summary of the invention
[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide a method for simultaneously extracting lithium and aluminum from clay-type lithium ore. The method directly destroys the structure of the clay-type lithium ore through pressurized alkaline leaching, and simultaneously leaches out lithium and aluminum elements; the leachate is then subjected to adsorption, desorption and carbon separation processes to obtain a lithium-rich solution and an aluminum hydroxide product, respectively, without the need for a roasting process, which greatly reduces production energy consumption, simplifies the process flow, and realizes the comprehensive utilization of lithium and aluminum resources in clay-type lithium ore.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] The present invention provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, the method comprising the following steps:
[0011] The clay-type lithium ore is mixed with an alkaline solution for pressurized alkaline leaching, and then a leachate is obtained by solid-liquid separation; the leachate is adsorbed by a lithium-extracting adsorbent to obtain a lithium-rich adsorbent and an adsorption residual liquid; the lithium-rich adsorbent is desorbed to obtain a lithium-rich solution; the adsorption residual liquid is subjected to carbon separation to obtain aluminum hydroxide.
[0012] The present invention firstly adopts a pressurized alkali leaching method without the need for a high-temperature roasting process. The Al-O-Si bond in the insoluble component aluminosilicate of the clay-type lithium ore is destroyed by alkali leaching, and the lithium-aluminum mineral wrapped in the clay-type lithium ore is released, thereby leaching lithium and aluminum elements to obtain a lithium-aluminum leachate. The lithium and aluminum elements in the leachate are then separated and utilized through adsorption, desorption and carbon separation processes in sequence. Compared with the traditional precipitation impurity removal method, the present invention has the advantages of less lithium loss and less alkali material consumption. The problem that the clay-type lithium ore is difficult to dissociate and the lithium-aluminum element is difficult to leach is solved, and the comprehensive utilization of lithium-aluminum resources in the clay-type lithium ore is realized under mild conditions, and the production energy consumption is low and the waste residue is small.
[0013] It is worth noting that the concentration of lithium in the lithium-rich solution obtained in the present invention is 150-240 mg / L, for example, it can be 150 mg / L, 180 mg / L, 200 mg / L, 220 mg / L or 240 mg / L.
[0014] Preferably, the clay-type lithium ore includes any one of diaspore, boehmite, kaolinite or chlorite, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of diaspore and boehmite, a combination of boehmite and kaolinite, or a combination of kaolinite and chlorite, etc.
[0015] Preferably, the lithium content in the clay-type lithium ore is 0.25-0.45wt%, for example, it can be 0.25wt%, 0.28wt%, 0.30wt%, 0.32wt%, 0.35wt%, 0.38wt%, 0.40wt%, 0.42wt% or 0.45wt%, etc.
[0016] Preferably, the aluminum content in the clay-type lithium ore is 22.50-34.50wt%, for example, it can be 22.50wt%, 24.50wt%, 26.50wt%, 28.50wt%, 30.50wt%, 32.50wt% or 34.50wt%.
[0017] Preferably, the potassium content in the clay-type lithium ore is 0.32-0.68wt%, for example, it can be 0.32wt%, 0.35wt%, 0.40wt%, 0.45wt%, 0.50wt%, 0.54wt%, 0.58wt%, 0.60wt%, 0.65wt% or 0.68wt%, etc.
[0018] Preferably, the titanium content in the clay-type lithium ore is 2.44-4.58wt%, for example, it may be 2.44wt%, 2.57wt%, 3.14wt%, 3.67wt%, 4.22wt% or 4.58wt%.
[0019] Preferably, the calcium content in the clay-type lithium ore is 0.47-0.65wt%, for example, it can be 0.47wt%, 0.50wt%, 0.55wt%, 0.58wt%, 0.60wt% or 0.65wt%.
[0020] Preferably, the magnesium content in the clay-type lithium ore is 0.10-0.30wt%, for example, it may be 0.10wt%, 0.15wt%, 0.20wt%, 0.25wt% or 0.30wt%.
[0021] Preferably, the iron content in the clay-type lithium ore is 2.67-3.05wt%, for example, it may be 2.67wt%, 2.78wt%, 2.82wt%, 2.87wt% or 3.05wt%.
[0022] Preferably, the alkaline solution comprises any one or a combination of at least two of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate or ammonia water, wherein typical but non-limiting combinations include a combination of potassium hydroxide and sodium hydroxide, a combination of sodium carbonate and potassium carbonate, or a combination of sodium hydroxide and ammonia water, etc.
[0023] Preferably, the alkaline solution comprises a combination of at least two alkaline solutions.
[0024] Preferably, the mass ratio of the solutes of the two alkaline solutions is (1-5):1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1 or 5:1, etc.
[0025] Preferably, the solute concentration of the alkaline solution is 15-65wt%, for example, it can be 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt% or 65wt%.
[0026] Due to the complex mineral phase of clay-type lithium ore, it is difficult to dissociate the clay-type lithium ore. The present invention further preferably comprises at least two alkaline solutions, and the mass ratio of the solutes of the two alkaline solutions is (1-5):1 and the solute concentration of the alkaline solution is 15-65wt%, so that the two or more alkaline solutions of a specific ratio can work synergistically, thereby further improving the leaching effect of lithium and aluminum elements in the clay-type lithium ore; if a single alkaline solution is used, the leaching ability of lithium and aluminum elements becomes poor, and only a single type of mineral phase can be dissociated, resulting in incomplete dissociation of the clay-type lithium ore; if the mass ratio of the two alkaline solutions is too low or too high, the effect is similar to that of using a single alkaline solution, that is, the synergistic effect is weakened, and the leaching rate of lithium and aluminum elements is relatively poor.
[0027] It is worth noting that the alkali solution described in the present invention can be a weak alkaline solution such as sodium carbonate, potassium carbonate or ammonia water. This is because under a specific combination ratio, the average ion activity coefficient in the weak alkaline medium system is increased, a higher reaction temperature is obtained at a lower vapor pressure, and the transfer flow characteristics are excellent, which enhances the reaction kinetics, thereby achieving simultaneous leaching of lithium and aluminum.
[0028] Preferably, the solid-to-liquid ratio of the clay-type lithium ore to the alkaline solution is 1:(5-15) g / mL, for example, it can be 1:5 g / mL, 1:6 g / mL, 1:7 g / mL, 1:8 g / mL, 1:9 g / mL, 1:10 g / mL, 1:10 g / mL, 1:11 g / mL, 1:12 g / mL, 1:13 g / mL, 1:14 g / mL or 1:15 g / mL, etc., preferably 1:(10-15) g / mL.
[0029] The present invention further preferably has a solid-liquid ratio of 1: (5-15) g / mL and a solute concentration of 15-65 wt% for the clay-type lithium ore and the alkaline solution, so that the clay-type lithium ore reacts fully with the alkaline solution, which is beneficial to the forward progress of lithium and aluminum elements in the leaching process, improves the leaching kinetics of lithium and aluminum elements, is adapted to the solute combination of the alkaline solution, further adjusts the viscosity of the reaction slurry, takes into account the high leaching rate and improves the filtration performance of the reaction slurry; if the solid-liquid ratio of the clay-type lithium ore and the alkaline solution is low, and the alkali concentration of the alkaline solution is low, it is not conducive to the leaching of lithium and aluminum elements, and the alkaline leaching effect is poor; if the solid-liquid ratio of the clay-type lithium ore and the alkaline solution is high, and the alkali concentration of the alkaline solution is high, the clay-type lithium ore cannot be fully contacted with the alkaline solution, the leaching of lithium and aluminum elements is insufficient, and the viscosity of the reaction slurry is too large, which is not conducive to subsequent filtering operations.
[0030] Preferably, the pressure of the pressurized alkali leaching is 0.15-0.5 MPa, for example, it can be 0.15 MPa, 0.2 MPa, 0.25 MPa, 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa or 0.5 MPa.
[0031] Preferably, the temperature of the pressurized alkali leaching is 150-240°C, for example, it can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C or 240°C, etc., preferably 150-195°C.
[0032] Preferably, the pressurized alkali leaching time is 0.5 to 2.5 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h or 2.5 h.
[0033] Preferably, the pressurized alkali leaching process is accompanied by stirring.
[0034] Preferably, the stirring speed is 150-300 r / min, for example, it can be 150 r / min, 170 r / min, 200 r / min, 220 r / min, 240 r / min, 260 r / min, 280 r / min or 300 r / min.
[0035] The present invention further optimizes the parameters of the pressurized alkali leaching process, for example, the pressurized alkali leaching temperature is further preferably 150-240°C, the time is 0.5-2.5h and the stirring speed is 150-300r / min; the parameters work together, so that the Al-O-Si bond in the aluminosilicate, a hardly soluble component in the clay-type lithium ore, is destroyed without high-temperature roasting, and the lithium aluminum mineral is released at the same time, and is fully in contact with the alkaline solution, thereby increasing the reaction rate, thereby obtaining a high lithium and aluminum leaching rate under mild conditions; if the temperature is too low, the time is too short or the speed is too low, the clay-type lithium ore cannot fully react with the alkaline solution, the reaction rate is reduced, and the lithium and aluminum elements cannot be fully leached, resulting in; if the temperature is too high, the time is too long or the speed is too high, the leaching effect of lithium and aluminum elements is not significantly improved, but instead causes greater energy consumption.
[0036] Preferably, the pressure leaching reactor comprises a homogeneous reactor.
[0037] Preferably, the clay-type lithium ore is pretreated before the mixing.
[0038] Preferably, the pretreatment comprises a grinding process.
[0039] Preferably, the grinding treatment includes grinding the clay-type lithium ore to a particle size of ≤0.074 mm, with a mass percentage of more than 85%, for example, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95%, etc.
[0040] Preferably, the equipment used for the grinding treatment includes any one of a ball mill, a planetary ball mill, a stirred mill or a sand mill, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of a ball mill and a planetary ball mill, a combination of a planetary ball mill and a stirred mill, or a combination of a stirred mill and a sand mill, etc.
[0041] Preferably, the rotation speed of the grinding process is 300-500 r / min, for example, it can be 300 r / min, 350 r / min, 400 r / min, 450 r / min or 500 r / min.
[0042] Preferably, the grinding treatment time is 60 to 180 min, for example, it can be 60 min, 80 min, 100 min, 120 min, 140 min, 160 min or 180 min.
[0043] The present invention further preferably subjects the clay-type lithium ore to grinding treatment before the mixing, and controls the rotation speed of the grinding treatment to 300-500 r / min and the time to 60-180 min, so as to break the clay-type lithium ore, increase the specific surface area, increase the contact area with the alkaline solution, and improve its reaction activity, thereby improving the leaching rate of lithium and aluminum elements.
[0044] Preferably, the concentration of lithium in the leaching solution is 150-240 mg / L, for example, 150 mg / L, 180 mg / L, 200 mg / L, 220 mg / L or 240 mg / L.
[0045] Preferably, the concentration of aluminum in the leaching solution is 1.5-18 g / L, for example, it can be 1.5 g / L, 2 g / L, 5 g / L, 8 g / L, 10 g / L, 12 g / L, 15 g / L or 18 g / L.
[0046] The adsorption comprises the step of passing the leaching solution through an adsorption column filled with a lithium-extracting adsorbent to adsorb the leaching solution, thereby obtaining an adsorption column filled with a lithium-rich adsorbent and adsorption residual liquid.
[0047] Preferably, the type of adsorption is dynamic adsorption.
[0048] Preferably, the lithium extraction adsorbent includes any one of a manganese ion sieve, an aluminum ion sieve or a titanium ion sieve, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of a manganese ion sieve and an aluminum ion sieve, a combination of an aluminum ion sieve and a titanium ion sieve, or a combination of a manganese ion sieve and a titanium ion sieve, etc.
[0049] Preferably, the adsorption temperature is 25-30°C, for example, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.
[0050] Preferably, the flow rate of the leachate during the adsorption process is 0.09-0.12 BV / min, for example, 0.09 BV / min, 0.1 BV / min, 0.11 BV / min or 0.12 BV / min.
[0051] The present invention further controls the flow rate of the leaching solution to be 0.09-0.12 BV / min, which is beneficial to the adsorption of lithium elements, prevents a portion of lithium from remaining in the leaching solution to cause lithium loss, and prevents the lithium elements in the residual leaching solution from causing the subsequent aluminum products to be impure.
[0052] Preferably, the penetration time of the adsorption is 8 to 12 minutes, for example, it can be 8 minutes, 9 minutes, 10 minutes, 11 minutes or 12 minutes.
[0053] Preferably, the adsorption equilibrium time is 18 to 22 minutes, for example, 18 minutes, 19 minutes, 20 minutes, 21 minutes or 22 minutes.
[0054] Preferably, the desorption comprises introducing a desorption liquid into an adsorption column filled with a lithium-rich adsorbent.
[0055] Preferably, the desorption liquid comprises hydrochloric acid.
[0056] Preferably, the concentration of the hydrochloric acid is 0.1-0.5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L.
[0057] Preferably, the flow rate of the desorption liquid is 0.09-0.12 BV / min, for example, it can be 0.09 BV / min, 0.1 BV / min, 0.11 BV / min or 0.12 BV / min.
[0058] Preferably, the desorption temperature is 25-30°C, for example, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.
[0059] Preferably, the desorption time is 18 to 22 minutes, for example, 18 minutes, 19 minutes, 20 minutes, 21 minutes or 22 minutes.
[0060] It is worth noting that the initial lithium concentration in the desorption solution is relatively low, so as to form a concentration difference with the lithium-rich adsorbent, which is beneficial to the diffusion of lithium and further to the occurrence of the desorption reaction.
[0061] Preferably, the carbon separation comprises introducing carbon dioxide gas into the adsorption residual liquid to obtain aluminum hydroxide precipitate.
[0062] Preferably, the flow rate of the carbon dioxide gas is 20-60 mL / min, for example, it can be 20 mL / min, 25 mL / min, 30 mL / min, 35 mL / min, 40 mL / min, 45 mL / min, 50 mL / min, 55 mL / min or 60 mL / min.
[0063] The present invention further preferably has a flow rate of the carbon dioxide gas of 20 to 60 mL / min, which is beneficial to reducing the pH of the adsorption residual liquid and further beneficial to the precipitation of aluminum hydroxide; if the flow rate of the carbon dioxide gas is too low, the yield of aluminum hydroxide will be reduced; if the flow rate of the carbon dioxide gas is too high, silicon will be entrained in the aluminum hydroxide, or dawsonite will be generated, affecting the purity of the product.
[0064] Preferably, the temperature of the carbon fraction is 30-60°C, for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C.
[0065] Preferably, the carbon fractionation time is 2 to 6 hours, for example, it can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours.
[0066] As a further preferred technical solution of the present invention, according to Figure 1 The process flow shown in the figure is carried out, and the method comprises the following steps:
[0067] (1) Pretreatment: grinding a clay-type lithium ore having a lithium content of 0.25 to 0.45 wt% and an aluminum content of 22.50 to 34.50 wt% at a rotation speed of 300 to 500 r / min for 60 to 180 min to obtain a reaction material having a particle size of ≤0.074 mm and a weight proportion of more than 85%;
[0068] (2) pressurized alkali leaching: at 150-240° C., 0.15-0.5 MPa and 150-300 r / min, the reaction material obtained in step (1) is mixed with an alkaline solution having a concentration of 15-65 wt % and subjected to pressurized alkali leaching for 0.5-2.5 h at a solid-liquid ratio of 1:(5-15) g / mL, and then solid-liquid separation is performed to obtain a leachate;
[0069] (3) Adsorption: The leachate obtained in step (2) is passed through an adsorption column filled with a lithium-extracting adsorbent at a flow rate of 0.09 to 0.12 BV / min at 25 to 30° C. to obtain an adsorption column filled with a lithium-rich adsorbent and an adsorption residual liquid; the penetration time of the adsorption is 8 to 12 minutes, and the equilibrium time is 18 to 22 minutes;
[0070] (4) desorption: at 25-30° C., a desorption liquid having a flow rate of 0.09-0.12 BV / min is introduced into the adsorption column containing the lithium-rich adsorbent obtained in step (3) for desorption for 18-22 minutes to obtain a lithium-rich solution;
[0071] (5) Carbon separation: introducing carbon dioxide gas at a flow rate of 20 to 60 mL / min into the adsorption residual liquid obtained in step (3) at 30 to 60° C. for 2 to 6 hours to obtain aluminum hydroxide;
[0072] Wherein, the alkaline solution comprises a combination of at least two alkaline solutions, and the mass ratio of the solutes of the two alkaline solutions is (1-5):1.
[0073] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0074] Compared with the prior art, the present invention has the following beneficial effects:
[0075] (1) The method for simultaneously extracting lithium and aluminum from clay-type lithium ore provided by the present invention destroys the structure of the clay-type lithium ore that is difficult to dissociate through a pressurized alkaline leaching process, exposing the lithium and aluminum minerals wrapped or intercalated in the clay-type lithium ore. The lithium and aluminum elements are simultaneously leached under mild conditions without the need for high-temperature roasting, thereby avoiding the use of high-concentration strong acid and eliminating waste residue discharge. In addition, the lithium and aluminum elements in the leachate are subsequently separated and utilized through adsorption, desorption and carbon separation processes to obtain corresponding products, thereby realizing the comprehensive utilization of the lithium and aluminum elements in the clay-type lithium ore.
[0076] (2) The method for simultaneously extracting lithium and aluminum from clay-type lithium ore provided by the present invention further improves the leaching rate of lithium and aluminum in clay-type lithium ore by further adjusting the components and content ratio of the alkaline solution, and matching the preferred solid-liquid ratio, temperature, time and rotation speed parameters. The leaching rate of lithium is as high as 89.31% or more, preferably as high as 90.23% or more, and the leaching rate of aluminum is as high as 85.1% or more, preferably as high as 90.12% or more; and the comprehensive recovery rate of lithium and aluminum is further improved by controlling the subsequent adsorption, desorption and carbon separation process conditions. The comprehensive recovery rate of lithium is as high as 81.47% or more, preferably as high as 90.07% or more, and the comprehensive recovery rate of aluminum is as high as 82.69% or more, preferably as high as 85.17% or more. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] Figure 1 The present invention provides a process flow chart of a method for simultaneously extracting lithium and aluminum from clay-type lithium ore. DETAILED DESCRIPTION
[0078] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0079] The lithium extraction adsorbent used in the following examples is a titanium-based lithium extraction adsorbent (G-100, Yunnan Gangfeng New Materials Co., Ltd.).
[0080] 1. Implementation
[0081] Example 1
[0082] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, the method comprising the following steps:
[0083] (1) Pretreatment: grinding a clay-type lithium ore having a lithium content of 0.33 wt% and an aluminum content of 24.50 wt% at a rotation speed of 400 r / min for 90 min to obtain a reaction material having a particle size of ≤0.074 mm and a weight proportion of 87%;
[0084] (2) pressurized alkali leaching: at 195° C. and 180 r / min, 10 g of the reaction material obtained in step (1) was mixed with 120 mL of a mixed solution of potassium hydroxide and sodium hydroxide with a total concentration of 45 wt % at a solid-liquid ratio of 1:12 g / mL, and pressurized alkali leaching was performed for 1.5 h under closed conditions (the pressure in the autoclave during the pressurized alkali leaching process was in the range of 0.3 to 0.45 MPa), wherein the mass ratio of potassium hydroxide to sodium hydroxide was 2.5:1; and then filtered to obtain a leachate;
[0085] (3) Adsorption: The leachate obtained in step (2) is passed through an adsorption column filled with a titanium-based lithium-extraction adsorbent at a flow rate of 0.1 BV / min at 28° C. to obtain an adsorption column filled with a lithium-rich adsorbent and an adsorption residual liquid; the penetration time of the adsorption is 10 min, and the equilibrium time is 20 min;
[0086] (4) Desorption: At 28° C., 0.3 mol / L hydrochloric acid at a flow rate of 0.1 BV / min was introduced into the adsorption column containing the lithium-rich adsorbent obtained in step (3) for desorption for 20 min to obtain a lithium-rich solution;
[0087] (5) Carbon separation: At 40° C., carbon dioxide gas at a flow rate of 40 mL / min was introduced into the adsorption residual liquid obtained in step (3) for 4 h to perform carbon separation to obtain aluminum hydroxide precipitate.
[0088] The metal elements and their contents in the clay-type lithium ore in this embodiment are shown in Table 1;
[0089] Table 1
[0090]
[0091] Example 2
[0092] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, the method comprising the following steps:
[0093] (1) Pretreatment: grinding a clay-type lithium ore having a lithium content of 0.25 wt% and an aluminum content of 22.50 wt% at a rotation speed of 300 r / min for 180 min to obtain a reaction material having a particle size of ≤0.074 mm and a weight proportion of 89%;
[0094] (2) pressurized alkali leaching: at 180° C. and 300 r / min, 10 g of the reaction material obtained in step (1) was mixed with 100 mL of a mixed solution of potassium hydroxide and sodium hydroxide with a total concentration of 20 wt % at a solid-liquid ratio of 1:10 g / mL, and pressurized alkali leaching was performed for 1 h under closed conditions (the pressure in the autoclave during the pressurized alkali leaching process was in the range of 0.15 to 0.35 MPa), wherein the mass ratio of potassium hydroxide to sodium hydroxide was 1:1; and then filtered to obtain a leachate;
[0095] (3) Adsorption: The leachate obtained in step (2) is passed through an adsorption column filled with a titanium-based lithium-extraction adsorbent at a flow rate of 0.09 BV / min at 25° C. to obtain an adsorption column filled with a lithium-rich adsorbent and an adsorption residual liquid; the penetration time of the adsorption is 12 min, and the equilibrium time is 22 min;
[0096] (4) Desorption: At 25° C., 0.2 mol / L hydrochloric acid at a flow rate of 0.09 BV / min was introduced into the adsorption column containing the lithium-rich adsorbent obtained in step (3) for desorption for 22 min to obtain a lithium-rich solution;
[0097] (5) Carbon separation: At 30° C., carbon dioxide gas at a flow rate of 20 mL / min was introduced into the adsorption residual liquid obtained in step (3) for carbon separation for 2 h to obtain aluminum hydroxide precipitate.
[0098] The metal elements and contents in the clay-type lithium ore in this embodiment are shown in Table 2;
[0099] Table 2
[0100]
[0101] Example 3
[0102] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, the method comprising the following steps:
[0103] (1) Pretreatment: grinding a clay-type lithium ore having a lithium content of 0.45 wt% and an aluminum content of 34.50 wt% at a rotation speed of 500 r / min for 60 min to obtain a reaction material having a particle size of ≤0.074 mm and a weight proportion of 95%;
[0104] (2) pressurized alkali leaching: at 150° C. and 150 r / min, 10 g of the reaction material obtained in step (1) was mixed with 150 mL of a mixed solution of potassium hydroxide and sodium hydroxide with a total concentration of 65 wt % at a solid-liquid ratio of 1:15 g / mL, and pressurized alkali leaching was performed for 2.5 h under closed conditions (the pressure in the autoclave during the pressurized alkali leaching process was in the range of 0.2 to 0.3 MPa), wherein the mass ratio of potassium hydroxide to sodium hydroxide was 5:1; and then filtered to obtain a leachate;
[0105] (3) Adsorption: The leachate obtained in step (2) is passed through an adsorption column filled with a titanium-based lithium-extraction adsorbent at a flow rate of 0.12 BV / min at 30° C. to obtain an adsorption column filled with a lithium-rich adsorbent and an adsorption residual liquid; the penetration time of the adsorption is 8 min, and the equilibrium time is 18 min;
[0106] (4) Desorption: at 30° C., 0.1 mol / L hydrochloric acid at a flow rate of 0.12 BV / min was introduced into the adsorption column containing the lithium-rich adsorbent obtained in step (3) for desorption for 18 min to obtain a lithium-rich solution;
[0107] (5) Carbon separation: At 60° C., carbon dioxide gas at a flow rate of 60 mL / min was introduced into the adsorption residual liquid obtained in step (3) for carbon separation for 6 h to obtain aluminum hydroxide precipitate.
[0108] The metal elements and contents in the clay-type lithium ore in this embodiment are shown in Table 3;
[0109] Table 3
[0110]
[0111] Example 4
[0112] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Embodiment 1 except that the mixed solution of potassium hydroxide and sodium hydroxide in the pressurized alkaline leaching process in step (2) is replaced by a mixed solution of sodium carbonate and potassium carbonate.
[0113] Example 5
[0114] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Embodiment 1 except that potassium hydroxide is replaced by potassium carbonate during the pressurized alkaline leaching process in step (2).
[0115] Example 6
[0116] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Example 1 except that the mass ratio of potassium hydroxide to sodium hydroxide in step (2) is 6:1.
[0117] Example 7
[0118] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Embodiment 1 except that the mass ratio of potassium hydroxide to sodium hydroxide in step (2) is 1:2.
[0119] Example 8
[0120] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Embodiment 1 except that potassium hydroxide is replaced by sodium hydroxide during the pressurized alkaline leaching process in step (2), that is, a single alkaline solution is used.
[0121] Example 9
[0122] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Example 1 except that the solid-to-liquid ratio of the reaction material to the alkaline solution in step (2) is 1:9 g / mL.
[0123] Example 10
[0124] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Example 1 except that the solid-to-liquid ratio of the reaction material to the alkaline solution in step (2) is 1:16 g / mL.
[0125] Embodiment 11
[0126] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Embodiment 1 except that the temperature of the pressurized alkaline leaching in step (2) is 200°C.
[0127] Example 12
[0128] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Embodiment 1 except that the temperature of the pressurized alkaline leaching in step (2) is 140°C.
[0129] Embodiment 13
[0130] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Example 1 except that the flow rate of the carbon dioxide gas in step (5) is 70 mL / min.
[0131] Embodiment 14
[0132] This embodiment provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is the same as that of Example 1 except that the flow rate of the carbon dioxide gas in step (5) is 15 mL / min.
[0133] 2. Comparison
[0134] Comparative Example 1
[0135] This comparative example provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore. Except that step (2) is not carried out under closed conditions, that is, without pressurization, the rest is the same as Example 1.
[0136] Comparative Example 2
[0137] This comparative example provides a method for simultaneously extracting lithium and aluminum from clay-type lithium ore, which is carried out by the method disclosed in CN116356159A. A large amount of NaOH solution needs to be added during the impurity removal process, which greatly increases the production cost. In addition, the separation of lithium and aluminum is insufficient, resulting in a low purity of the product lithium carbonate.
[0138] 3. Test Results
[0139] The lithium and aluminum contents in the leaching solution obtained in step (2) in the above embodiment and comparative example, the lithium content in the lithium-rich solution obtained in step (4) and the aluminum content in the aluminum hydroxide precipitate obtained in step (5) were measured by inductively coupled plasma emission spectrometry (ICP); and the leaching rate and comprehensive recovery rate of lithium and aluminum in the clay-type lithium ore were calculated according to the following formulas. The results are shown in Table 4;
[0140] Lithium leaching rate = lithium content in leaching solution / (mass of clay-type lithium ore raw material*mass fraction of raw material lithium);
[0141] Aluminum leaching rate = aluminum content in leaching solution / (mass of clay-type lithium ore raw material*mass fraction of raw material aluminum);
[0142] Comprehensive lithium recovery rate = lithium content in lithium-rich solution / (mass of clay-type lithium ore raw material*mass fraction of raw material lithium);
[0143] Comprehensive aluminum recovery rate = aluminum content in aluminum hydroxide product / (mass fraction of clay-type lithium ore raw material*mass fraction of raw aluminum).
[0144] Table 4
[0145]
[0146] From Table 4, we can see the following points:
[0147] (1) It can be seen from Examples 1 to 5 that the method of the present invention is to mix clay-type lithium ore with an alkaline solution for pressurized alkaline leaching. After sufficient reaction, the leaching rate of lithium in the clay-type lithium ore is as high as 90.23% or more, and the leaching rate of aluminum is as high as 90.12% or more; and by subsequent adsorption, desorption and carbon separation, the comprehensive recovery rate of lithium in the clay-type lithium ore is as high as 90.07% or more, and the comprehensive recovery rate of aluminum is as high as 85.17% or more.
[0148] (2) Combining Example 1 with Examples 6 to 7, it can be seen that when the mass ratio of potassium hydroxide to sodium hydroxide in step (2) of Example 6 and Example 7 is too high or too low, the lithium leaching rate drops to below 96.24%, and the aluminum leaching rate drops to below 89.54% after testing; further, the comprehensive recovery rate of lithium drops to below 91.54%, and the comprehensive recovery rate of aluminum drops to below 85.31%. It can be seen that the present invention further prefers that the mass ratio of the solutes in the two alkaline solutions is (1 to 5): 1, which further promotes the transformation of the mineral phase in the clay-type lithium ore, makes the encapsulated lithium aluminum minerals more easily exposed, and further improves the leaching rate of lithium and aluminum and their comprehensive recovery rate.
[0149] (3) Combining Example 1 and Example 8, it can be seen that when Example 8 uses a single alkaline solution for pressurized alkali leaching, the lithium leaching rate is 90.48%, and the aluminum leaching rate is 91.57%; the comprehensive recovery rate of lithium is 90.12%, and the comprehensive recovery rate of aluminum is 86.24%. It can be seen that the present invention further preferably uses a combination of at least two alkaline solutions during the pressurized alkali leaching process, which can further improve the leaching effect of lithium and aluminum in clay-type lithium ore.
[0150] (4) Combining Example 1 with Examples 9 to 10, it can be seen that when the solid-liquid ratio of the reaction material to the alkaline solution in step (2) of Example 9 and Example 10 is low or high, the clay-type lithium ore cannot fully contact with the alkaline solution, the mineral phase conversion is incomplete, the solute concentration is too low or the viscosity of the reaction slurry is too high to be conducive to subsequent filtration, and the leaching rate and recovery rate are both reduced. It can be seen that the present invention further preferably has a solid-liquid ratio of the reaction material to the alkaline solution of 1: (10 to 15) g / mL, which further improves the leaching of lithium and aluminum in the clay-type lithium ore.
[0151] (5) Combining Example 1 with Examples 11 to 12, it can be seen that when the temperature of the pressurized alkali leaching in Example 11 is high, the leaching rate of lithium and aluminum is not significantly improved, while when the temperature of the pressurized alkali leaching in Example 12 is low, due to the incomplete mineral phase change of the clay-type lithium ore and the insufficient release of the lithium-aluminum ore phase, the leaching rate of lithium and aluminum is significantly reduced; thus, it can be seen that the present invention further preferably sets the temperature of the pressurized alkali leaching to 150 to 195°C, which can further improve the leaching of clay-type lithium and aluminum, and the heat energy consumption is relatively small.
[0152] (6) Combining Example 1 with Examples 13 to 14, it can be seen that when the flow rate of the carbon dioxide gas in step (5) of Example 13 is 70 mL / min, the comprehensive recovery rate of aluminum is 86.41%; when the flow rate of the carbon dioxide gas in step (5) of Example 14 is 15 mL / min, the comprehensive recovery rate of aluminum is 84.63%; thus, it can be seen that the present invention further prefers that the flow rate of the carbon dioxide gas is 20 to 60 mL / min, which is more conducive to the formation of aluminum hydroxide products.
[0153] (7) It can be seen from the combination of Example 1 and Comparative Examples 1 to 2 that when Comparative Example 1 is not carried out in a closed environment, the clay-type lithium ore structure is difficult to dissociate, and the acid solution cannot fully transform its ore phase at a relatively low temperature, resulting in a lithium leaching rate of only 70.25% and an aluminum leaching rate of only 60.45%. The method provided in Comparative Example 2 has a large amount of impurities in the impurity removal process, the product purity is low, and a large amount of alkali solution is consumed, resulting in a high production cost.
[0154] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for simultaneously extracting lithium and aluminum from clay-type lithium ore, characterized in that: The method comprises the following steps: The clay-type lithium ore is mixed with an alkaline solution for pressurized alkaline leaching, and then a leachate is obtained by solid-liquid separation; the leachate is adsorbed by a lithium-extracting adsorbent to obtain a lithium-rich adsorbent and an adsorption residual liquid; the lithium-rich adsorbent is desorbed to obtain a lithium-rich solution; the adsorption residual liquid is subjected to carbon separation to obtain aluminum hydroxide.
2. The method according to claim 1, characterized in that The clay-type lithium ore includes any one of diaspore, boehmite, kaolinite or lithium chlorite, or a combination of at least two thereof; Preferably, the content of lithium in the clay-type lithium ore is 0.25-0.45wt%; Preferably, the aluminum content in the clay-type lithium ore is 22.50-34.50wt%.
3. The method according to claim 1 or 2, characterized in that: The alkaline solution includes any one or a combination of at least two of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate or ammonia water; Preferably, the alkaline solution comprises a combination of at least two alkaline solutions; Preferably, the mass ratio of the solutes of the two alkaline solutions is (1-5):1; Preferably, the solute concentration of the alkaline solution is 15 to 65 wt %; Preferably, the solid-liquid ratio of the clay-type lithium ore to the alkaline solution is 1:(5-15) g / mL, preferably 1:(10-15) g / mL.
4. The method according to any one of claims 1 to 3, characterized in that: The pressure of the pressurized alkali leaching is 1.5-2MPa; Preferably, the temperature of the pressurized alkali leaching is 150-240°C, preferably 150-195°C; Preferably, the pressurized alkali leaching time is 0.5 to 2.5 hours; Preferably, the pressurized alkali leaching process is accompanied by stirring; Preferably, the stirring speed is 150-300 r / min.
5. The method according to any one of claims 1 to 4, characterized in that: The clay-type lithium ore is pre-treated before the mixing; Preferably, the pretreatment includes grinding treatment; Preferably, the grinding process comprises grinding the clay-type lithium ore to a particle size of ≤0.074 mm with a mass percentage of more than 85%; Preferably, the equipment used for the grinding process includes any one of a ball mill, a planetary ball mill, a stirred mill or a sand mill, or a combination of at least two thereof; Preferably, the rotation speed of the grinding process is 300-500 r / min; Preferably, the grinding treatment time is 60 to 180 minutes.
6. The method according to any one of claims 1 to 5, characterized in that: The concentration of lithium in the leaching solution is 150-240 mg / L; Preferably, the concentration of aluminum in the leaching solution is 1.5-18 g / L.
7. The method according to any one of claims 1 to 6, characterized in that: The adsorption comprises the following steps: the leaching solution is adsorbed through an adsorption column filled with a lithium-extracting adsorbent to obtain an adsorption column filled with a lithium-rich adsorbent and an adsorption residual liquid; Preferably, the type of adsorption is dynamic adsorption; Preferably, the adsorption temperature is 25-30°C; Preferably, the flow rate of the leachate during the adsorption process is 0.09 to 0.12 BV / min; Preferably, the penetration time of the adsorption is 8 to 12 minutes; Preferably, the adsorption equilibrium time is 18 to 22 minutes.
8. The method according to any one of claims 1 to 7, characterized in that: The desorption comprises passing a desorption liquid into an adsorption column filled with a lithium-rich adsorbent; Preferably, the flow rate of the desorption liquid is 0.09 to 0.12 BV / min; Preferably, the desorption temperature is 25-30°C; Preferably, the desorption time is 18 to 22 minutes.
9. The method according to any one of claims 1 to 8, characterized in that: The carbon separation comprises introducing carbon dioxide gas into the adsorption residual liquid to obtain aluminum hydroxide precipitation; Preferably, the flow rate of the carbon dioxide gas is 20 to 60 mL / min; Preferably, the temperature of the carbon fraction is 30-60°C; Preferably, the carbon fractionation time is 2 to 6 hours.
10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) Pretreatment: grinding a clay-type lithium ore having a lithium content of 0.25 to 0.45 wt% and an aluminum content of 22.50 to 34.50 wt% at a rotation speed of 300 to 500 r / min for 60 to 180 min to obtain a reaction material having a particle size of ≤0.074 mm and a weight proportion of more than 85%; (2) pressurized alkali leaching: at 150-240° C., 0.15-0.5 MPa and 150-300 r / min, the reaction material obtained in step (1) is mixed with an alkaline solution having a concentration of 15-65 wt % and subjected to pressurized alkali leaching for 0.5-2.5 h at a solid-liquid ratio of 1:(5-15) g / mL, and then solid-liquid separation is performed to obtain a leachate; (3) Adsorption: The leachate obtained in step (2) is passed through an adsorption column filled with a lithium-extracting adsorbent at a flow rate of 0.09 to 0.12 BV / min at 25 to 30° C. to obtain an adsorption column filled with a lithium-rich adsorbent and an adsorption residual liquid; the penetration time of the adsorption is 8 to 12 minutes, and the equilibrium time is 18 to 22 minutes; (4) desorption: at 25 to 30° C., a desorption liquid having a flow rate of 0.09 to 0.12 BV / min is introduced into the adsorption column containing the lithium-rich adsorbent obtained in step (3) for desorption for 18 to 22 min to obtain a lithium-rich solution; (5) Carbon separation: introducing carbon dioxide gas at a flow rate of 20 to 60 mL / min into the adsorption residual liquid obtained in step (3) at 30 to 60° C. for 2 to 6 hours to obtain aluminum hydroxide; Wherein, the alkaline solution comprises a combination of at least two alkaline solutions, and the mass ratio of the solutes of the two alkaline solutions is (1-5):1.
Citation Information
Cited By
Comprehensive utilization method of clay type lithium ore
CN121204431A
Comprehensive utilization method of clay type lithium ore
CN121204431B