Production method of longitudinal-crack-free peritectic high-aluminum steel thick plate blank

By controlling the composition of molten steel and the production process, the problem of longitudinal cracking of peritectic high-aluminum steel was solved, and the production of thick slabs of peritectic high-aluminum steel without longitudinal cracks was achieved, which significantly improved the surface quality and production efficiency of the cast slab and reduced economic losses. .

CN118773500APending Publication Date: 2024-10-15HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410567625.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Peritectic high-aluminum steel is prone to surface defects such as longitudinal cracks during the pouring process, resulting in reduced billet yield and increased supply costs. Existing technology cannot effectively solve this problem.

Method used

By controlling the content of S and P elements in the molten steel, using special protective powder for peritectic high-aluminum steel, adjusting the pouring temperature and the insertion depth of the immersed nozzle, controlling the δ phase remaining rate, and performing KR molten iron desulfurization and molten iron pre-dephosphorization in the production process. , converter double slag smelting and LF and VD refining processes to reduce the unevenness of aluminum content and carbon content, reduce the impact of steel slag reaction, and improve the lubrication effect and inflow of protective slag.

Benefits of technology

The longitudinal cracking rate of peritectic high-aluminum steel is significantly reduced from 16% to 0, which improves the surface quality of the cast slab, reduces economic losses, and meets the performance requirements of subsequent finished products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773500A_ABST
    Figure CN118773500A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of a longitudinal-crack-free peritectic high-aluminum steel thick slab, and belongs to the technical field of metallurgy. The method comprises the working procedures of KR molten iron pre-desulfurization, molten iron pre-dephosphorization, converter double-slag smelting, LF refining, VD refining and thick slab continuous casting. The converter double-slag smelting procedure is divided into a dephosphorization period and a decarbonization period; the method comprises the following steps: performing narrow composition control on C, Mn and Cr elements of a steel grade according to a control upper limit, and performing narrow composition control on Al, Ti, S, P and N elements according to a control lower limit; covering slag special for peritectic high-aluminum steel is used in the thick slab continuous casting procedure; other steel types with low crack sensitivity are used as casting starting steel types, and peritectic high-aluminum steel is poured in a second furnace of the continuous casting times where the peritectic high-aluminum steel is located; the insertion depth of the submersed nozzle is controlled according to the upper limit in the pouring process, and the superheat degree is controlled to be 15-25 DEG C; according to the method, the peritectic high-aluminum steel thick plate blank without longitudinal crack surface defects can be produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for producing a peritectic high-aluminum steel thick slab without longitudinal cracks. Background Art

[0002] Peritectic high-aluminum steel refers to a steel with an acid-soluble aluminum mass fraction of more than 0.5% and a carbon content near the peritectic point. Due to the peritectic reaction and the slag reaction of the high-aluminum steel protective slag, high-aluminum steel is prone to surface defects such as longitudinal cracks during the casting process, which is a major problem that plagues major steel mills. Due to the existence of this defect, the high-aluminum steel ingot yield rate is greatly reduced, the supply cost is increased, and the development of this steel is restricted.

[0003] The Chinese patent application with application number 201410525736.6 discloses "a method for producing high-aluminum steel". The high-aluminum steel referred to in the invention is high-carbon high-aluminum steel, and its carbon content is not within the range of peritectic steel. Therefore, this method is not suitable for the production of peritectic high-aluminum steel continuous casting billets. The Chinese patent application with application number 201711012923.9 discloses "a method for continuous casting of subperitectic steel slabs". The steel involved in the invention is not high-aluminum steel, so this method is not suitable for the production of peritectic high-aluminum steel continuous casting billets.

[0004] In the prior art, there is no effective method to solve the above technical problems of peritectic high-aluminum steel. Summary of the invention

[0005] To solve the above technical problems, the present invention provides a production method for peritectic high-aluminum steel thick slab without longitudinal cracks by combining component design and production process improvement according to the causes of longitudinal cracks on the surface of peritectic high-aluminum steel.

[0006] The reasons for the longitudinal cracks on the surface of peritectic high-aluminum steel: Due to the high aluminum content of this steel, it reacts with the protective slag in the crystallizer, causing significant changes in the composition and properties of the protective slag, increasing the viscosity and melting point, and the poor flow of protective slag. The newly cast billet is heated unevenly in the crystallizer, which can easily lead to uneven thickness of the billet shell in some areas, thereby causing cracks. At the same time, the carbon content of peritectic high-aluminum steel is often near the peritectic point, and a phase transition process from δ phase to γ ​​phase will occur in the crystallizer, the volume of molten steel will shrink, and the growth of the primary billet shell will be uneven, which further aggravates the crack sensitivity of peritectic high-aluminum steel, and surface defects such as longitudinal cracks are prone to appear on the surface of the billet.

[0007] The design idea of ​​the present invention: (1) In order to reduce the crack sensitivity of peritectic high-aluminum steel, the elements such as S and P in the molten steel that will reduce the grain boundary strength are controlled. The present invention adopts KR molten iron desulfurization, molten iron pre-dephosphorization, and converter double slag smelting processes to stably control the S and P contents in the finished product to less than 0.003%.

[0008] (2) The use of special protective slag for peritectic high-aluminum steel can effectively reduce defects such as longitudinal cracks on the surface of the casting billet caused by the peritectic reaction caused by the composition characteristics of peritectic high-aluminum steel and the steel slag reaction, thereby improving the surface quality of the continuous casting billet.

[0009] (3) Due to the existence of slag reaction, when the molten steel flow rate on the surface of the crystallizer decreases, the renewal rate of the slag interface will decrease, which will lead to the local enrichment of A12O3 produced by the slag interface reaction. The enrichment of A12O3 reduces the CaO / Al2O3 of the protective slag in this area, and the ability of the protective slag to adsorb and dissolve A12O3 is further reduced, thus forming a vicious circle. Ultimately, the melting temperature of the protective slag increases, the viscosity increases, the lubrication ability of the protective slag decreases, and even slag strips are generated, affecting the inflow of the protective slag. In order to promote the melting of the protective slag on the surface of the crystallizer and enhance the lubrication effect of the protective slag, the insertion depth of the submerged nozzle during the casting process of peritectic high-aluminum steel is controlled according to the upper limit, that is, 115-125mm, and the pouring temperature is increased at the same time to control the superheat at 15-25℃.

[0010] (4) When peritectic high-aluminum steel solidifies in a crystallizer, a peritectic reaction will occur. After the peritectic reaction is completed, the less the residual rate of the δ phase is, the smaller the shrinkage of the ingot caused by the transformation of the δ phase to the γ phase in the subsequent solidification process, the more uniform the growth of the primary ingot shell, and the lower the incidence of surface defects. For a specific type of steel, in order to meet the performance of its subsequent finished product, the chemical composition of each element has its control range. In the original production process, each element is controlled according to the middle limit of its composition control range. In the present invention, in order to reduce the residual rate of the δ phase and thus reduce the incidence of surface defects in the ingot, the C and Mn elements of this steel are narrowly controlled according to the upper control limit, and the Al, Ti, S, P, and N elements are narrowly controlled according to the lower control limit.

[0011] (5) The production of peritectic high-aluminum steel is scheduled after the current casting of other steel grades, making full use of the heat of the previous furnace of molten steel to preheat the continuous casting equipment so that the molten steel can be cooled evenly and stably in the crystallizer.

[0012] Based on the above research and design ideas, the present invention provides a method for producing a peritectic high-aluminum steel thick slab without longitudinal cracks, wherein the chemical composition and mass percentage of the peritectic high-aluminum steel are C: 0.080-0.120%, Mn: 1.85-2.20%, Al S : 0.500~0.800%, Cr: 0.20~0.30%, Ti: 0.010~0.025%, P≤0.003%, S≤0.003%, N≤45ppm and other residual elements; its production method includes the following steps: (1) KR hot metal desulfurization process: ensure that the outgoing hot metal [S] ≤ 0.01wt%; (2) Hot metal pre-dephosphorization process: pre-dephosphorization treatment is carried out before adding iron to the converter to ensure that the outlet hot metal [P] ≤ 0.010wt%; (3) Converter double slag smelting process: the double slag method is adopted, with converter smelting dephosphorization period and converter smelting decarburization period; the slag discharge volume in the dephosphorization period is 60-70%, the composition and mass percentage of the molten steel at the end of smelting are [C]: 0.020-0.040%, [S] ≤ 0.008%, [P] ≤ 0.003%, and the end temperature is 1640-1660℃; (4) LF and VD refining process: the target composition and mass percentage of the molten steel at the time of leaving the station are [C]=0.120%, [Als]=0.500%, [Mn]=2.20%, [Cr]=0.30%, [Ti]=0.010%, [S]≤0.003%, [P]≤0.003%, [N]≤0.0045%; that is, the C and Mn elements of this steel are narrowly controlled according to the upper control limit, and the Al, Ti, S, P, and N elements are narrowly controlled according to the lower control limit; (5) Thick slab continuous casting process: The tundish uses a carbon-free low-silicon covering agent, and the protective slag uses a special protective slag for peritectic high-aluminum steel; the superheat of the tundish steel is controlled at 15-25°C; the insertion depth of the immersion nozzle is controlled at 115-125mm; when casting peritectic high-aluminum steel, other steel grades with lower crack sensitivity are used as the opening steel grade, and the casting of peritectic high-aluminum steel is arranged in the second furnace of the continuous casting sequence; the main components and weight ratio of the special protective slag for peritectic high-aluminum steel are SiO2: 30.0-35.0%, CaO: 20.0-24.0%, MgO: 2.0-3.5%, Al2O3: 3.5-5.0%, Na2O: 5.0-8.0%, F: 8.5-10.0%, C: 7.5-10.0%.

[0013] Furthermore, in the KR molten iron desulfurization process, the slag is pre-scraped before desulfurization to make the exposed surface of the molten iron ≥20%; after desulfurization, the slag on the surface of the molten iron is scraped off to make the exposed surface of the molten iron ≥90%.

[0014] Furthermore, in the converter double-slag smelting process, lime is added during the converter smelting dephosphorization period according to the basicity of 1.2 to 1.5, the smelting end temperature is 1370 to 1400° C., and [P] in the semi-steel is ≤0.003%.

[0015] Furthermore, in the converter double-slag smelting process, the basicity of the final slag during the converter smelting decarburization period is controlled to be 3.5-4.0, the FeO mass percentage in the final slag is ≤20%, the smelting end point temperature is 1640-1660°C, the end point [O] content is 500-650ppm, and the end point [P] content is ≤0.003%.

[0016] Furthermore, in the converter smelting process, the converter steelmaking adopts a front and rear double-block process, the front block adopts a slag blocking plug, and the rear block adopts a slide plate and a slag blocking mark to block the slag, and the lower slag thickness is ≤20mm.

[0017] Furthermore, in the thick slab continuous casting process, the thickness of the cast slab is 300-330 mm, the water distribution of the crystallizer adopts a slow cooling mode, the water volume on the wide surface is 4500-4800 L / min, and the flow rate on the narrow surface is 400-450 L / min.

[0018] The beneficial effects of adopting the above technical solution are: (1) The present invention improves the use effect of the protective slag, reduces the crack sensitivity of the steel grade, and realizes the control of the surface cracks of the ingot by controlling the S and P element content of the molten steel, the superheat, the insertion depth of the immersion nozzle, the composition of the protective slag of the continuous casting crystallizer, etc.

[0019] (2) The present invention reduces the longitudinal crack rate of peritectic high-aluminum steel from 16% to 0, significantly reducing the economic losses caused by quality reasons. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The surface quality map of the continuous casting slab produced by the prior art; Figure 2 This is the surface quality diagram of the continuous casting billet of Example 1; Figure 3 This is the surface quality diagram of the continuous casting billet in Example 2. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below with reference to the embodiments.

[0022] Examples 1-10 The production process of the peritectic high-aluminum steel thick slab without longitudinal cracks of the present invention is: KR hot metal desulfurization → hot metal pre-dephosphorization → converter double slag smelting → LF refining and VD refining → thick slab continuous casting process. The present invention has no special restrictions on the processing capacity of each process, and the specific operation steps are as follows: (1) KR hot metal desulfurization process After the molten iron ladle enters the station, the slag is pre-scraped to make the exposed surface of the molten iron ≥20%. The desulfurizer uses lime powder. After desulfurization, the slag on the surface of the molten iron is scraped clean, the exposed surface of the molten iron is ≥90%, and the molten iron [S] is ≤0.010wt% to avoid rephosphorization caused by deep desulfurization of reducing slag in the refining process. The process parameter control of each embodiment is shown in Table 1.

[0023] (2) Hot metal pre-dephosphorization process Dephosphorization pretreatment is performed before adding iron to the converter, and nitrogen is used as a carrier to transport dephosphorizing agents such as CaO and fluorite into the ladle for stirring and dephosphorization to ensure that the outlet molten iron [P] ≤ 0.010wt%. The process parameter control of each embodiment is shown in Table 1.

[0024]

[0025] (3) Converter double slag smelting process A. Converter dephosphorization period smelting: average temperature of molten iron entering the furnace is 1280-1330℃, S≤0.010wt%, P≤0.010wt%; lime is added according to basicity of 1.2-1.5, smelting end temperature is 1370-1400℃, [P]≤0.003wt% in the end semi-steel, and the slag discharge amount during dephosphorization period is 60-70%. The process parameter control of each embodiment is shown in Table 2.

[0026]

[0027] B. Converter decarburization period smelting: the basicity of the final blowing slag is controlled at 3.5-4.0, the FeO mass percentage in the final slag is ≤20%, the smelting end temperature is 1640-1660°C, the end [O] content is 500-650ppm, the components and mass percentages in the end molten steel are [C]: 0.022-0.040%, [S]≤0.008%, [P]≤0.003%; the process parameter control of each embodiment is shown in Table 3.

[0028] C. The converter tapping adopts the front and rear double-block process, the front block adopts the slag blocking plug, the rear block adopts the slide plate and the slag blocking mark to block the slag, and the slag is controlled by infrared slag detection, and the slag thickness is ≤20mm. The process parameter control of each embodiment is shown in Table 3.

[0029]

[0030] (4) LF and VD refining process A. Due to the high aluminum content of this steel grade, in order to prevent the increase of the [Si] content in the molten steel caused by the reaction between the molten steel [Al] and the SiO2 in the refined slag, it is necessary to control the SiO2 in the LF refined slag to ≤8.0%; in order to ensure the desulfurization effect, the slag is deoxidized through the aluminum line segment, and the end slag sample TFe+MnO≤1.0%; B. After the VD process starts, the lowest vacuum degree is drawn and the VD bottom blowing gas flow rate is controlled to 80~100 Nm 3 / h. After 15 min of vacuum cycle, the temperature is measured and samples are taken for component analysis; C. According to the sampling analysis results, the composition of the molten steel is adjusted to a narrow range. The C, Mn, and Cr elements are controlled according to the upper control limits, and the Al, Ti, S, P, and N elements are controlled according to the lower control limits. The target composition and mass percentage of the molten steel at the time of leaving the station are [C]=0.120%, [Als]=0.500%, [Mn]=2.20%, [Cr]=0.30%, [Ti]=0.010%, [S]≤0.003%, [P]≤0.003%, and [N]≤0.0045%.

[0031] The LF and VD refining process parameter control of each embodiment is shown in Table 4.

[0032]

[0033] (5) Thick slab continuous casting process A. The superheat of the tundish steel is controlled at 15-25℃, and the tundish uses a carbon-free and low-silicon covering agent; B. The insertion depth of the immersion nozzle is controlled at 115-125mm; C. The protective slag uses a special protective slag for peritectic high aluminum steel, and its main components and weight ratio are SiO2: 30.0-35.0%, CaO: 20.0-24.0%, MgO: 2.0-3.5%, Al2O3: 3.5-5.0%, Na2O: 5.0-8.0%, F: 8.5-10.0%, C: 7.5-10.0%; D. The crystallizer water distribution adopts slow cooling mode, with a wide surface water volume of 4500-4800L / min and a narrow surface flow rate of 400-450L / min; the ingot thickness is 300mm-330mm; when pouring peritectic high-aluminum steel, other steel grades are used as the opening steel grade, and the pouring of peritectic high-aluminum steel is arranged in the second furnace of its pouring sequence.

[0034] The control parameters of the thick slab continuous casting process in each embodiment are shown in Tables 5 and 6.

[0035] The chemical composition and mass percentage of the peritectic high aluminum steel continuous casting billet produced by the above process are shown in Table 7.

[0036]

[0037]

[0038]

[0039] The continuous casting ingots produced by the above process showed no defects such as surface longitudinal cracks after cold inspection, and the longitudinal crack rate of peritectic high-aluminum steel was reduced from 16% to 0, which can well meet the requirements of the subsequent hot rolling process for the casting ingot quality.

Claims

1. A method for producing a peritectic high-aluminum steel thick slab without longitudinal cracks, It is characterized in that The chemical composition and mass percentage of the peritectic high aluminum steel are C: 0.080-0.120%, Mn: 1.85-2.20%, Al S : 0.500~0.800%, Cr:0.20~0.30%, Ti: 0.010~0.025%, P≤0.003%, S≤0.003%, N≤45ppm and other residual elements; its production method includes the following steps: (1) KR hot metal desulfurization process: ensure that the outgoing hot metal [S] ≤ 0.01wt%; (2) Hot metal pre-dephosphorization process: pre-dephosphorization treatment is carried out before adding iron to the converter to ensure that the outlet hot metal [P] ≤ 0.010wt%; (3) Converter double slag smelting process: the double slag method is adopted, with converter smelting dephosphorization period and converter smelting decarburization period; the slag discharge volume in the dephosphorization period is 60-70%, the composition and mass percentage of the molten steel at the end of smelting are [C]: 0.020-0.040%, [S] ≤ 0.008%, [P] ≤ 0.003%, and the end temperature is 1640-1660℃; (4) LF and VD refining process: the target composition and mass percentage of the molten steel at the time of leaving the station are [C]=0.120%, [Als]=0.500%, [Mn]=2.20%, [Cr]=0.30%, [Ti]=0.010%, [S]≤0.003%, [P]≤0.003%, [N] ≤0.0045%; that is, the C, Mn and Cr elements of this steel are narrowly controlled according to the upper control limit, and the Al, Ti, S, P and N elements are narrowly controlled according to the lower control limit; (5) Thick slab continuous casting process: The tundish uses a carbon-free low-silicon covering agent, and the protective slag uses a special protective slag for peritectic high-aluminum steel; the superheat of the tundish steel is controlled at 15-25°C; the insertion depth of the immersion nozzle is controlled at 115-125mm; when casting peritectic high-aluminum steel, other steel grades with low crack sensitivity are used as the first casting steel grade, and the casting of peritectic high-aluminum steel is arranged in the second furnace of the continuous casting run; the main components and weight ratio of the special protective slag for peritectic high-aluminum steel are SiO 2 :30.0~35.0%, CaO: 20.0~24.0%, MgO: 2.0~3.5%, Al 2 O 3 :3.5~5.0%,Na 2 O: 5.0~8.0%, F: 8.5~10.0%, C: 7.5~10.0%.

2. The method for producing a peritectic high aluminum steel thick slab without longitudinal cracks according to claim 1, It is characterized in that In the KR hot metal desulfurization process, slag is pre-scraped before desulfurization to make the exposed surface of the hot metal ≥20%; after desulfurization, the slag on the surface of the hot metal is scraped off to make the exposed surface of the hot metal ≥90%.

3. The method for producing a peritectic high aluminum steel thick slab without longitudinal cracks according to claim 2, It is characterized in that In the converter double-slag smelting process, lime is added during the converter smelting dephosphorization period according to the basicity of 1.2 to 1.5, the smelting end temperature is 1370 to 1400° C., and [P] in the semi-steel is ≤0.003%.

4. The method for producing a peritectic high aluminum steel thick slab without longitudinal cracks according to claim 3, It is characterized in that In the converter double-slag smelting process, the basicity of the final slag during the converter smelting decarburization period is controlled to be 3.5-4.0, the FeO mass percentage in the final slag is ≤20%, the smelting end point temperature is 1640-1660°C, the end point [O] content is 500-650ppm, and the end point [P] content is ≤0.003%.

5. The method for producing a peritectic high aluminum steel thick slab without longitudinal cracks according to claim 4, It is characterized in that In the converter smelting process, the converter steel is tapped using a front and rear double-block process, the front block uses a slag blocking plug, and the rear block uses a slide plate and a slag blocking mark to block the slag, and the lower slag thickness is ≤20mm.

6. The method for producing a peritectic high aluminum steel thick slab without longitudinal cracks according to any one of claims 1 to 5, It is characterized in that In the thick slab continuous casting process, the thickness of the cast slab is 300-330 mm, the water distribution of the crystallizer adopts a slow cooling mode, the water volume on the wide surface is 4500-4800 L / min, and the flow rate on the narrow surface is 400-450 L / min.