Element modified aluminide cladding coating and preparation method thereof
By adding components such as La2O3, NH4Cl, Pt and Hf to the aluminide coating, and using the plasma cladding process to prepare the aluminide cladding coating, the problem of insufficient oxidation resistance of the aluminide coating in high temperature environments has been solved, significantly improving It improves the anti-oxidation and thermal corrosion resistance of the coating and is suitable for large boilers and complex-shaped workpieces.
Patent Information
- Application Number
- CN202410782618.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The existing aluminide coating has insufficient oxidation resistance in high-temperature environments, causing oxidation and corrosion problems on the inner walls of boiler pipes, affecting the operating costs and material life of the unit.
The element-modified aluminide cladding coating is prepared using a plasma cladding process. By adding components such as La2O3, NH4Cl, Pt and Hf to the cladding powder, the penetration and activation of the coating and the pinning of the oxide film are improved. Effect, enhance antioxidant and thermal corrosion resistance.
It significantly improves the bonding strength and oxidation resistance of the aluminide cladding coating and the base material, extends the service life of the coating, and increases the oxidation resistance by 20-74 times in a high-temperature water vapor environment.
Smart Images

Figure CN118773602A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material surface alloying and coating preparation, and specifically relates to an element-modified aluminide cladding coating and a preparation method thereof. Background Art
[0002] In the thermal power generation industry, oxidation and corrosion of the inner wall of the flow pipe is the main factor leading to boiler non-stop accidents, causing the operating cost and material cost of the unit to increase by more than 20%; therefore, research and development of anti-oxidation technology suitable for the inner wall surface of the pipe used in boiler units has important practical significance.
[0003] Research shows that aluminide coatings have significant effects in solving the problems of oxidation corrosion, wear, and high-temperature ablation of the inner wall of pipelines; however, with the increase in power and service life of generator sets, single aluminide coatings face the problem of insufficient oxidation resistance. Based on this, it is necessary to develop a new type of aluminide anti-oxidation coating with better service performance and suitable for various complex-shaped workpieces with large aspect ratios and other complex shapes, as well as its preparation process. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art and provide a new technical solution for an element-modified aluminide cladding coating and a preparation method thereof.
[0005] According to a first aspect of the present invention, there is provided a
[0006] According to a first aspect of the present invention, there is provided a method for preparing an element-modified aluminide cladding coating, comprising the following steps:
[0007] Step S1, the solid phase components are 50-80% FeAl, 10-
[0008] 35% Al, 2-5% La2O3, 3-6% Pt, 3-6% Hf and 1-5% NH4Cl are stirred, ball-milled and dried to prepare a cladding powder; wherein the sum of the mass percentages is 100%;
[0009] Step S2, cleaning the surface of the workpiece to be plated, and pouring a sufficient amount of cladding powder into the feed port of the ion cladding device;
[0010] Step S3, placing the workpiece to be plated under an inert atmosphere, using an ion cladding device to spray cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating after cooling;
[0011] Step S4, treating the cladding residue.
[0012] Optionally, in step S1, FeAl, Al, Pt, and Hf are all in powder form, and FeAl, Al, Pt, and Hf are all sieved through a 1000-mesh sieve.
[0013] Optionally, in step S1, the cladding powder is obtained by wet-grinding a solid phase component with a planetary ball mill and then drying it.
[0014] Optionally, when the solid phase component is wet-milled in a planetary ball mill, the wet-milling medium is anhydrous ethanol, the ball milling speed is 350-400 rpm, the time is 12-24 h, and the drying conditions are vacuum drying at 80-120° C. for 12-24 h.
[0015] Optionally, the process parameters of plasma cladding are as follows:
[0016] The cladding current is 80-120A, the feed rate is 18-22g / min, the scanning rate is 20-40cm / min, the nozzle height is 8-12mm, the rotation speed is 2-5r / min, the ion gas flow rate is 0.2-0.3L / min, and the shielding gas flow rate is 18-20L / min.
[0017] Optionally, the inert gas in the inert atmosphere is Ar or N2.
[0018] Optionally, in step S2, the surface of the workpiece to be plated is cleaned with a high-pressure water gun for 5 minutes and then rinsed with alcohol or acetone.
[0019] Optionally, the cladding residue is treated, including:
[0020] Use a high-pressure water gun to wash away the cladding residue on the surface of the workpiece and let it dry naturally.
[0021] Optionally, in step S3, the thickness of the aluminide cladding coating is 0.94-2.35 mm.
[0022] According to a second aspect of the present invention, there is provided an element-modified aluminide cladding coating, which is prepared by the preparation method described in the first aspect and comprises a solid phase component, wherein the solid phase component comprises the following components in mass percentage:
[0023] 50-80% FeAl, 10-35% Al, 2-5% La2O3, 3-6% Pt, 3-6% Hf and 1-5% NH4Cl; wherein the sum of the mass percentages is 100%.
[0024] A technical effect of the present invention is:
[0025] In the embodiment of the present application, the preparation method of the element-modified aluminide cladding coating adopts a plasma cladding process to prepare the aluminide cladding coating. Since the plasma cladding process has the advantages of concentrated heat, short action time, and small thermal influence in the cladding area, the aluminide cladding coating has a high bonding strength with the parent material. At the same time, the preparation method of the rare earth element-modified aluminide cladding coating prepares the aluminide cladding coating through an integrated production line, which not only has high production efficiency and controllable thickness of the aluminide cladding coating, but also has high process repeatability and is extremely practical.
[0026] In addition, by adding La2O3 and NH4Cl to the cladding powder components, the infiltration and activation effects are achieved, which significantly improves the infiltration rate and coating quality; by introducing Pt and Hf to co-modify the aluminide coating, oxidation products can be produced to pin the coating oxide film, thereby simultaneously improving the antioxidant and heat corrosion resistance of the parent material.
[0027] Furthermore, the addition of rare earth oxides can pin the grain boundaries, refine the matrix structure, improve the surface hardness, and enhance the bonding strength between the coating and the parent material in the form of second phase precipitation on the basis of halide-promoted diffusion. At the same time, the introduction of Pt element modification can provide a channel for Al elements to form dense oxides, inhibit or reduce the external diffusion of alloy elements, accelerate the transformation of θ-Al2O3 to α-Al2O3, improve the film-base bonding, effectively inhibit internal oxidation and internal sulfidation, and enhance the thermal corrosion resistance of the coating. Moreover, the introduction of Hf element modification can aggregate at the oxide grain boundaries and hinder further oxidation of the parent material. Its oxidation product HfO2 can pin the oxide film, enhance the oxide's anti-stripping performance, and thus enhance the coating's antioxidant and anti-oxidation capabilities. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A method for preparing an element-modified aluminide cladding coating according to an embodiment of the present invention;
[0029] Figure 2 Schematic diagram of the cross-sectional morphology of an aluminide cladding coating according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application.
[0031] The embodiments of the present application will be described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be construed as limitations on the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0032] The term "first" or "second" in the specification and claims of this application may include one or more of the features explicitly or implicitly. In the description of this application, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the objects connected before and after are in an "or" relationship.
[0033] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0034] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0035] According to a first aspect of the present invention, Figure 1 As shown, a method for preparing an element-modified aluminide cladding coating is provided, comprising the following steps:
[0036] Step S1, solid phase components are stirred, ball-milled, and dried according to mass percentage of 50-80% FeAl (infiltration source), 10-35% Al (infiltration source), 2-5% La2O3 (infiltration catalyst), 3-6% Pt (modifier), 3-6% Hf (modifier) and 1-5% NH4Cl (catalyst) to prepare cladding powder; wherein the sum of the mass percentages is 100%;
[0037] Step S2, cleaning the surface of the workpiece to be plated, and pouring a sufficient amount of cladding powder into the feed port of the ion cladding device;
[0038] Step S3, placing the workpiece to be plated under an inert atmosphere, using an ion cladding device to spray cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating after cooling;
[0039] Step S4, treating the cladding residue.
[0040] In the embodiment of the present application, the preparation method of the element-modified aluminide cladding coating adopts a plasma cladding process to prepare the aluminide cladding coating. Since the plasma cladding process has the advantages of concentrated heat, short action time, and small thermal influence in the cladding area, the aluminide cladding coating has a high bonding strength with the parent material. At the same time, the preparation method of the rare earth element-modified aluminide cladding coating prepares the aluminide cladding coating through an integrated production line, which not only has high production efficiency and controllable thickness of the aluminide cladding coating, but also has high process repeatability and is extremely practical.
[0041] In addition, by adding La2O3 and NH4Cl to the cladding powder components, the infiltration and activation effects are achieved, which significantly improves the infiltration rate and coating quality; by introducing Pt and Hf to co-modify the aluminide coating, oxidation products can be produced to pin the coating oxide film, thereby simultaneously improving the antioxidant and heat corrosion resistance of the parent material.
[0042] Furthermore, the addition of rare earth oxides can pin the grain boundaries, refine the matrix structure, improve the surface hardness, and enhance the bonding strength between the coating and the parent material in the form of second phase precipitation on the basis of halide-promoted diffusion. At the same time, the introduction of Pt element modification can provide a channel for Al elements to form dense oxides, inhibit or reduce the external diffusion of alloy elements, accelerate the transformation of θ-Al2O3 to α-Al2O3, improve the film-base bonding, effectively inhibit internal oxidation and internal sulfidation, and enhance the thermal corrosion resistance of the coating. Moreover, the introduction of Hf element modification can aggregate at the oxide grain boundaries and hinder further oxidation of the parent material. Its oxidation product HfO2 can pin the oxide film, enhance the oxide's anti-stripping performance, and thus enhance the coating's antioxidant and anti-oxidation capabilities.
[0043] Optionally, in step S1, FeAl, Al, Pt, and Hf are all in powder form, and FeAl, Al, Pt, and Hf are all sieved through a 1000-mesh sieve.
[0044] In the above embodiment, it helps to ensure that each component is dispersed more evenly and finely, and remove impurities and particles therein, thereby better ensuring the cladding effect of the aluminide cladding coating.
[0045] Optionally, in step S1, the cladding powder is obtained by wet-grinding a solid phase component with a planetary ball mill and then drying it.
[0046] In the above embodiment, a cladding powder in which each component is fully and evenly mixed can be obtained, which helps to better ensure the quality of the aluminide cladding coating during the cladding process.
[0047] Optionally, when the solid phase component is wet-milled in a planetary ball mill, the wet-milling medium is anhydrous ethanol, the ball milling speed is 350-400 rpm, the time is 12-24 h, and the drying conditions are vacuum drying at 80-120° C. for 12-24 h.
[0048] In the above-mentioned embodiment, the wet grinding method of the solid phase component is relatively reasonable, which helps to ensure the uniform fineness of the cladding powder.
[0049] Optionally, the process parameters of plasma cladding are as follows:
[0050] The cladding current is 80-120A, the feed rate is 18-22g / min, the scanning rate is 20-40cm / min, the nozzle height is 8-12mm, the rotation speed is 2-5r / min, the ion gas flow rate is 0.2-0.3L / min, and the shielding gas flow rate is 18-20L / min.
[0051] In the above embodiment, the various parameters of the plasma cladding process are reasonably set, so that the cladding process has the advantages of concentrated heat, short action time, and small thermal impact in the cladding area, thereby making the bonding strength between the aluminide cladding coating and the parent material higher.
[0052] Optionally, the inert gas in the inert atmosphere is Ar or N2. Using chemically stable Ar or N2 to provide an inert atmosphere helps to ensure that the workpiece to be plated is not oxidized during the cladding process.
[0053] Optionally, in step S2, the surface of the workpiece to be plated is cleaned with a high-pressure water gun for 5 minutes and then rinsed with alcohol or acetone.
[0054] In the above embodiment, oil stains, dust, etc. on the surface of the workpiece to be plated can be well removed, and the oxide scale can be removed, and it can be rinsed with alcohol or acetone to provide a neat and metallic surface for subsequent cladding, thereby helping to ensure the strength and stability of the combination between the workpiece surface and the aluminide cladding coating.
[0055] Optionally, the cladding residue is treated, including:
[0056] Use a high-pressure water gun to wash away the cladding residue on the surface of the workpiece and let it dry naturally.
[0057] In the above embodiment, the cladding residue can be thoroughly processed to ensure the cleanliness of the workpiece surface.
[0058] Optionally, in step S3, the thickness of the aluminide cladding coating is 0.94-2.35 mm, which makes the aluminide cladding coating have good metallurgical bonding performance, so that the aluminide cladding coating has high bonding strength with the parent material.
[0059] According to a second aspect of the present invention, there is provided an element-modified aluminide cladding coating, which is prepared by the preparation method described in the first aspect and comprises a solid phase component, wherein the solid phase component comprises the following components in mass percentage:
[0060] 50-80% FeAl, 10-35% Al, 2-5% La2O3, 3-6% Pt, 3-6% Hf and 1-5% NH4Cl; wherein the sum of the mass percentages is 100%.
[0061] In the above-mentioned embodiment, by adding La2O3 and NH4Cl to the cladding powder components, the effects of catalysis and activation are achieved, which significantly improves the infiltration rate and coating quality; by introducing Pt and Hf to co-modify the aluminide coating, oxidation products can be produced to pin the coating oxide film, thereby simultaneously improving the antioxidant and heat corrosion resistance of the parent material.
[0062] Furthermore, the addition of rare earth oxides can pin the grain boundaries, refine the matrix structure, improve the surface hardness, and enhance the bonding strength between the coating and the parent material in the form of second phase precipitation on the basis of halide-promoted diffusion. At the same time, the introduction of Pt element modification can provide a channel for Al elements to form dense oxides, inhibit or reduce the external diffusion of alloy elements, accelerate the transformation of θ-Al2O3 to α-Al2O3, improve the film-base bonding, effectively inhibit internal oxidation and internal sulfidation, and enhance the thermal corrosion resistance of the coating. Moreover, the introduction of Hf element modification can aggregate at the oxide grain boundaries and hinder further oxidation of the parent material. Its oxidation product HfO2 can pin the oxide film, enhance the oxide's anti-flaking performance, and thus enhance the coating's antioxidant capacity.
[0063] In the embodiments of the present application, the element-modified aluminide cladding coating and its preparation method prepare an aluminide cladding coating with a thickness of 0.94-2.35 mm and good metallurgical bonding under the conditions of adjusting the main process parameters such as the cladding powder composition and plasma cladding parameters; the aluminide cladding coating obtained by the present invention has an antioxidant capacity that is 20-64 times higher than that of the parent material in a 600°C pure water vapor environment, and an antioxidant capacity that is 24-74 times higher than that of the parent material in a 650°C pure water vapor environment, which indicates that the aluminide cladding coating prepared by the method of the present invention effectively improves the antioxidant capacity of the alloy parent material in a water vapor environment.
[0064] Example 1
[0065] Step S1, weighing each component of the solid phase component according to mass percentage, including 50% FeAl, 35% Al, 2% NH4Cl, 3% La2O3, 5% Pt and 5% Hf; placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 hours, and vacuum drying at 100°C for 24 hours to obtain the cladding powder.
[0066] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0067] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar or N2, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 120A, feed rate of 18g / min, scanning rate of 25cm / min, nozzle height of 10mm, rotation speed of 2r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0068] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0069] Example 2-Example 11
[0070] The cladding process of Example 2 to Example 11 is the same as that of Example 1. Example 1 to Example 11 maintain the same ratio of the penetrant component. The specific conditions are detailed in Table 1. Table 1 is the specific parameters of Example 1 to Example 11 of the preparation method of the element-modified aluminide cladding coating. According to the preparation steps in the above Example 1 and the specific preparation parameters in the table, aluminide cladding coatings of different thicknesses can be obtained.
[0071] Table 1
[0072]
[0073] By analyzing and studying the above-mentioned embodiments, the thickness of the infiltration layer is measured to be about 0.94-2.35 mm. The specific results are shown in Table 1. The cross-sectional morphology of the cladding coating prepared in Example 1 is as follows: Figure 2 As shown in Table 1 and the cross-sectional morphology, it is found that the diffusion layer has a uniform structure, moderate thickness, sufficient diffusion of Al atoms, and a good metallurgical bond between the diffusion layer and the matrix, and is not easy to fall off.
[0074] Example 12
[0075] Step S1, weighing each component of the solid phase component according to mass percentage, including 80% FeAl, 10% Al, 1% NH4Cl, 3% La2O3, 3% Pt and 3% Hf; placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 350rpm, the time is 24h, and vacuum drying at 100°C for 24h to obtain the cladding powder.
[0076] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0077] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar or N2, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 80A, feed rate of 20g / min, scanning rate of 40m / min, nozzle height of 12mm, rotation speed of 3r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0078] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0079] Example 13
[0080] Step S1, weighing each component of the solid phase component according to mass percentage, including 60% FeAl, 25% Al, 2% NH4Cl, 3% La2O3, 5% Pt and 5% Hf; placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 hours, and vacuum drying at 100°C for 24 hours to obtain the cladding powder.
[0081] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0082] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 100A, feed rate of 18g / min, scanning rate of 35m / min, nozzle height of 10mm, rotation speed of 3r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0083] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0084] Embodiment 14
[0085] Step S1, weighing each component of the solid phase component according to mass percentage, including 70% FeAl, 15% Al, 2% NH4Cl, 3% La2O3, 5% Pt and 5% Hf; placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 hours, and vacuum drying at 100°C for 24 hours to obtain the cladding powder.
[0086] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0087] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 120A, feed rate of 20g / min, scanning rate of 35m / min, nozzle height of 10mm, rotation speed of 2r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0088] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0089] Embodiment 15
[0090] Step S1, weighing each component of the solid phase component according to mass percentage, including 65% FeAl, 16% Al, 5% NH4Cl, 5% La2O3, 6% Pt and 3% Hf; placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 hours, and vacuum drying at 100°C for 24 hours to obtain the cladding powder.
[0091] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0092] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 120A, feed rate of 20g / min, scanning rate of 35m / min, nozzle height of 10mm, rotation speed of 2r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0093] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0094] Example 16
[0095] Step S1, weighing each component of the solid phase component according to mass percentage, including 65% FeAl, 16% Al, 5% NH4Cl, 5% La2O3, 3% Pt and 6% Hf; placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 hours, and vacuum drying at 100°C for 24 hours to obtain the cladding powder.
[0096] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0097] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 120A, feed rate of 20g / min, scanning rate of 35m / min, nozzle height of 10mm, rotation speed of 2r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0098] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0099] In the embodiments of the present application, the aluminide cladding coating prepared by the preparation method of the element-modified aluminide cladding coating is suitable for austenitic steel and high-temperature alloy components used in large boilers, oil and gas field transportation pipelines and other workpieces with large aspect ratios and various complex shapes. It is not only highly practical, has a high diffusion rate, and excellent membrane-base bonding strength, but also has excellent industrial mass production benefits.
[0100] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing an element-modified aluminide cladding coating, characterized in that: The steps include: Step S1, solid phase components are stirred, ball-milled, and dried according to mass percentage of 50-80% FeAl, 10-35% Al, 2-5% La2O3, 3-6% Pt, 3-6% Hf, and 1-5% NH4Cl to prepare a cladding powder; wherein the sum of the mass percentages is 100%; Step S2, cleaning the surface of the workpiece to be plated, and pouring a sufficient amount of cladding powder into the feed port of the ion cladding device; Step S3, placing the workpiece to be plated under an inert atmosphere, using an ion cladding device to spray cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating after cooling; Step S4, treating the cladding residue.
2. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: In step S1, FeAl, Al, Pt, and Hf are all in powder form, and FeAl, Al, Pt, and Hf are all sieved through a 1000-mesh sieve.
3. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: In step S1, the cladding powder is obtained by wet-grinding the solid phase components with a planetary ball mill and then drying them.
4. The method for preparing the element-modified aluminide cladding coating according to claim 3, characterized in that: When the solid phase components are wet-milled in a planetary ball mill, the wet-milling medium is anhydrous ethanol, the ball milling speed is 350-400 rpm, the time is 12-24 h, and the drying conditions are vacuum drying at 80-120° C. for 12-24 h.
5. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: The process parameters of plasma cladding are as follows: The cladding current is 80-120A, the feed rate is 18-22g / min, the scanning rate is 20-40cm / min, the nozzle height is 8-12mm, the rotation speed is 2-5r / min, the ion gas flow rate is 0.2-0.3L / min, and the shielding gas flow rate is 18-20L / min.
6. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: The inert gas in the inert atmosphere is Ar or N2.
7. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: In step S2, the surface of the workpiece to be plated is cleaned with a high-pressure water gun for 5 minutes and then rinsed with alcohol or acetone.
8. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: Treatment of cladding residues, including: Use a high-pressure water gun to wash away the cladding residue on the surface of the workpiece and let it dry naturally.
9. The method for preparing the element-modified aluminide cladding coating according to claim 1, characterized in that: In step S3, the thickness of the aluminide cladding coating is 0.94-2.35 mm.
10. An element-modified aluminide cladding coating, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9, comprising a solid phase component, wherein the solid phase component comprises the following components in percentage by weight: 50-80% FeAl, 10-35% Al, 2-5% La2O3, 3-6% Pt, 3-6% Hf and 1-5% NH4Cl; wherein the sum of the mass percentages is 100%.
Citation Information
Patent Citations
Method of producing (FeAl+Cr7C3) / (gamma Fe, Ni) composite coating
CN101245461A
Preparation method for Pt-Zr modified aluminide coating
CN107268044A
Method for improving high-temperature oxidization resistance of calorized coating
CN107858640A
Process of using ion fusion covering technology for preparing metal surface coating
CN110424006A
Thermophilic corrosion-resistance coating
CN1121538A
Cited By
Modifier component of aluminum-silicon cladding coating and modification method
CN120006282A