FeCrAl composite coating for zirconium alloy surface as well as preparation method and application of FeCrAl composite coating

The FeCrAl composite coating is formed on the surface of the zirconium alloy through ultra-high-speed laser cladding technology, which solves the problems of insufficient uniformity and bonding force of the traditional coating, significantly improves the high-temperature water vapor oxidation performance and anti-oxidation performance of the zirconium alloy surface, and delays the Core degradation process.

CN118773604AActive Publication Date: 2024-10-15NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410895480.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-15
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The traditional FeCrAl coating has poor uniformity and insufficient bonding force on the surface of zirconium alloy, making it difficult to meet the requirements of high-temperature water vapor oxidation performance and radiation resistance. In particular, there are technical difficulties in arc-shaped surface deposition, and it is easy to peel off in harsh environments.

Method used

Ultra-high-speed laser cladding technology is used to form a FeCrAl composite coating on the surface of a zirconium alloy substrate, including a metallurgical bonding layer and a FeCrAl cladding layer. The metallurgical bonding layer is composed of Fe-Zr and Cr-Zr solid solution. The FeCrAl cladding layer has a body-centered cubic shape. Structure, with a grain size of 10-30 μm, preheating the zirconium alloy matrix reduces cracks and unmelted particles and improves bonding strength.

Benefits of technology

The zirconium alloy surface coating achieves high binding force, low dilution rate, uniform and fine structure, significantly improves the resistance to high-temperature water vapor oxidation, reduces the risk of damage, forms Cr and Al oxide films to effectively protect the matrix, and enhances the resistance to High temperature oxidation corrosion performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773604A_ABST
    Figure CN118773604A_ABST
Patent Text Reader

Abstract

The invention discloses a FeCrAl composite coating for a zirconium alloy surface as well as a preparation method and application of the FeCrAl composite coating. The FeCrAl composite coating comprises a metallurgical bonding layer and a FeCrAl cladding layer which are sequentially formed on the surface of a base body, and the FeCrAl composite coating is formed by cladding FeCrAl alloy on the surface of a zirconium alloy substrate through the ultra-high-speed laser cladding technology. Wherein in the direction away from the surface of the base body, the content of Fe, Cr and Al elements in the metallurgical bonding layer is gradually increased, and the metallurgical bonding layer is mainly composed of a Fe-Zr solid solution and a Cr-Zr solid solution. The FeCrAl composite coating can form metallurgical bonding with a matrix, the coating structure is uniform and fine, the reaction speed of a cladding material and water vapor at a high temperature can be reduced, the reactor core degradation process is delayed, and the zirconium alloy pipe has excellent high-temperature oxidation resistance and good mechanical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of accident fault-tolerant fuel coatings, and in particular relates to a FeCrAl composite coating for a zirconium alloy surface, a preparation method and an application thereof. Background Art

[0002] Nuclear energy is a clean, low-carbon, safe and efficient strategic energy source, and it occupies a vital position in the future energy market. Zirconium (Zr) and its alloys have outstanding nuclear properties, such as small thermal neutron absorption cross section, excellent radiation resistance, high thermal conductivity, good mechanical properties, etc., so the concept of accident tolerant fuel (ATF) was proposed. The research and development of zirconium alloy surface coatings with high resistance to water vapor oxidation, corrosion resistance, wear resistance, hydrogen absorption resistance and radiation resistance is the international mainstream direction for the development of ATF surface enhanced zirconium alloy cladding materials. FeCrAl alloy has attracted much attention among candidate materials for accident tolerance due to its high thermal conductivity and excellent high-temperature oxidation resistance.

[0003] Traditional coating preparation technologies, such as spraying, have poor quality uniformity for thin coatings, and physical vapor deposition technology has technical difficulties in uniform deposition on the curved surface of the cladding tube. The key point is that the coating and the substrate are both physically bonded interfaces, and long-term service in harsh environments faces the risk of coating peeling, which cannot meet production needs. Therefore, in view of the limitations of the existing FeCrAl coating structure and preparation process, it is an urgent problem to provide a high-resistance coating that can be used on the surface of the fuel cladding and its preparation method. Summary of the invention

[0004] The main purpose of the present invention is to provide a FeCrAl composite coating for the surface of a zirconium alloy, and a preparation method and application thereof. The prepared FeCrAl composite coating has good bonding strength with the zirconium alloy, a low dilution rate, a fine coating structure, and a uniform coating thickness, so that the coating has good resistance to high-temperature water vapor oxidation and can reduce the risk of damage to the zirconium alloy cladding in an accident environment.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] An embodiment of the present invention provides a FeCrAl composite coating for a zirconium alloy surface, wherein the FeCrAl composite coating comprises a metallurgical bonding layer and a FeCrAl cladding layer sequentially formed on a substrate surface, wherein the FeCrAl composite coating is formed by cladding FeCrAl alloy on the surface of a zirconium alloy substrate using an ultra-high-speed laser cladding technology; wherein in a direction away from the substrate surface, the contents of Fe, Cr, and Al elements in the metallurgical bonding layer gradually increase, the metallurgical bonding layer is mainly composed of a Fe-Zr solid solution and a Cr-Zr solid solution, and the main phase of the FeCrAl cladding layer comprises an α-Fe-based solid solution alloy having a body-centered cubic structure; and the grain size of the FeCrAl cladding layer is 10 to 30 μm.

[0007] The embodiment of the present invention also provides a method for preparing the aforementioned FeCrAl composite coating on the surface of a zirconium alloy, which comprises:

[0008] Providing a zirconium alloy substrate;

[0009] Preheating the zirconium alloy substrate to 200-500° C.;

[0010] Furthermore, the FeCrAl alloy is clad on the surface of a zirconium alloy substrate using an ultra-high-speed laser cladding technology to obtain a FeCrAl composite coating on the surface of the zirconium alloy.

[0011] The embodiment of the present invention also provides the use of the aforementioned FeCrAl composite coating in the protection of curved surface parts.

[0012] The embodiment of the present invention further provides a fuel cladding device, which includes a zirconium alloy tube and a FeCrAl composite coating prepared by the aforementioned preparation method.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] (1) The present invention prepares a FeCrAl composite coating on the surface of a zirconium alloy tube by an ultra-high-speed laser cladding method. The coating forms a metallurgical bond with the substrate. Compared with traditional cladding, the thickness of the dilution layer between the coating and the substrate is smaller, and the thickness of the dilution layer is 20 to 80 μm. At the same time, the treated zirconium alloy tube has excellent high-temperature oxidation resistance, lower surface roughness and higher hardness.

[0015] (2) The present invention preheats the zirconium alloy tube before preparing the coating to reduce cracks formed due to too fast solidification speed, avoid the phenomenon of aggravated corrosion during high-temperature oxidation caused by cracks, and reduce the size of unmelted particles;

[0016] (3) The FeCrAl composite coating prepared by the present invention can be oxidized in water vapor at 1200°C for 60 minutes and maintain the integrity of the coating structure without large-scale peeling. The good bonding force improves the oxidation resistance of the coating in a steam environment and avoids falling off in a high-temperature water vapor environment. At the same time, the Cr and Al oxide films formed on the surface of the coating during the oxidation process can effectively block the diffusion of oxygen from the external environment to the coating and the substrate, effectively protecting the substrate, with low oxidation weight gain, and showing good resistance to high-temperature oxidation corrosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1a-1b is a cross-sectional SEM image of the FeCrAl composite coating prepared in Example 1 of the present invention;

[0019] Figure 2 is a grain size diagram of the FeCrAl composite coating prepared in Example 1 of the present invention;

[0020] Figure 3 is an X-ray diffraction pattern of the FeCrAl composite coating prepared in Example 1 of the present invention;

[0021] Figure 4 is a scratch surface image of the FeCrAl composite coating prepared in Example 1 of the present invention;

[0022] Figure 5a-Figure 5b Surface profile and roughness curves of FeCrAl coatings prepared in Example 1 and Comparative Example 2 of the present invention;

[0023] Figure 6 is a graph showing the weight gain of the FeCrAl composite coating obtained in Example 1 of the present invention when subjected to oxidation in high-temperature water vapor at 1200°C;

[0024] Figure 7 The cross-sectional SEM and EDS images of the FeCrAl composite coating prepared in Example 1 of the present invention after being oxidized in high-temperature water vapor at 1200° C. for 60 minutes;

[0025] Figure 8 is the surface X-ray diffraction pattern of the FeCrAl composite coating prepared in Example 1 of the present invention after being oxidized for 60 minutes;

[0026] Fig. 9is a cross-sectional SEM image of the FeCrAl composite coating prepared in Example 2 of the present invention;

[0027] Fig.10 is a cross-sectional SEM image of the FeCrAl composite coating prepared in Example 3 of the present invention;

[0028] Fig.11 is a cross-sectional SEM image of the FeCrAl coating prepared in Comparative Example 1 of the present invention;

[0029] Fig.12 This is a cross-sectional SEM image of the FeCrAl coating prepared in Comparative Example 1 of the present invention after being oxidized in high-temperature water vapor at 1200° C. for 60 minutes;

[0030] Figure 13a-13b is a cross-sectional SEM image of the FeCrAl coating prepared in Comparative Example 2 of the present invention;

[0031] Fig.14 This is a cross-sectional SEM image of the FeCrAl coating prepared in Comparative Example 2 of the present invention after being oxidized in high-temperature water vapor at 1200° C. for 60 minutes;

[0032] Fig.15 is a cross-sectional SEM image of the FeCrAl coating prepared in Comparative Example 3 of the present invention;

[0033] Fig.16 It is a digital image of the surface of the FeCrAl coating prepared in Comparative Example 4 of the present invention;

[0034] Fig.17 is an oxidation weight gain curve of the FeCrAl coating prepared in Comparative Example 5 of the present invention;

[0035] Fig.18 It is a hardness diagram of the FeCrAl coating prepared in Comparative Example 5 of the present invention. DETAILED DESCRIPTION

[0036] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution mainly adopts ultra-high-speed laser cladding technology to prepare metal anti-oxidation coatings. The bonding strength of the coatings is greatly improved compared with the coatings prepared by traditional methods. At the same time, the mechanical properties are relatively excellent.

[0037] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Specifically, as one aspect of the technical solution of the present invention, a FeCrAl composite coating for a zirconium alloy surface comprises a metallurgical bonding layer and a FeCrAl cladding layer sequentially formed on the surface of a substrate, wherein the FeCrAl composite coating is formed by cladding FeCrAl alloy on the surface of a zirconium alloy substrate using ultra-high-speed laser cladding technology; wherein, in a direction away from the substrate surface, the contents of Fe, Cr, and Al elements in the metallurgical bonding layer gradually increase, the metallurgical bonding layer is mainly composed of a Fe-Zr solid solution and a Cr-Zr solid solution, and the main phase of the FeCrAl cladding layer comprises an α-Fe-based solid solution alloy having a body-centered cubic structure; and the grain size of the FeCrAl cladding layer is 10 to 30 μm.

[0039] The FeCrAl composite coating in the present invention can form a metallurgical bond with the substrate, the coating has a uniform and fine structure, excellent bonding force and high strength, can reduce the reaction rate of the cladding material with water vapor at high temperature, reduce the heat generated by cladding oxidation, delay the core degradation process, and make the zirconium alloy tube have better high-temperature oxidation resistance and mechanical properties.

[0040] In some preferred embodiments, the FeCrAl cladding layer includes the following components calculated by mass percentage: 68 wt % Fe, 25 wt % Cr and 7 wt % Al.

[0041] In some preferred embodiments, the thickness of the metallurgical bonding layer is 0 to 60 μm.

[0042] In some preferred embodiments, the FeCrAl cladding layer has a thickness of 20 to 50 μm.

[0043] In some preferred embodiments, the α-Fe based solid solution alloy includes a Fe—Cr solid solution.

[0044] Furthermore, the content of Fe-Cr solid solution in the FeCrAl coating is 74-88wt%.

[0045] In some preferred embodiments, the zirconium alloy substrate includes a Zr-4 alloy tube, but is not limited thereto.

[0046] Furthermore, the length of the Zr-4 alloy tube is 300 to 400 mm.

[0047] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned FeCrAl composite coating on the surface of a zirconium alloy, comprising:

[0048] Providing a zirconium alloy substrate;

[0049] Preheating the zirconium alloy substrate to 200-500° C.;

[0050] Furthermore, the FeCrAl alloy is clad on the surface of a zirconium alloy substrate using an ultra-high-speed laser cladding technology to obtain a FeCrAl composite coating on the surface of the zirconium alloy.

[0051] In some preferred embodiments, the average particle size of the FeCrAl alloy is 10-30 μm.

[0052] In some preferred embodiments, the purity of the FeCrAl alloy is above 99.9 wt %.

[0053] In some preferred embodiments, the FeCrAl alloy includes the following components calculated by mass percentage: 68 wt % Fe, 25 wt % Cr and 7 wt % Al.

[0054] In some preferred embodiments, the preparation method specifically includes: using ultra-high-speed laser cladding technology to clad the FeCrAl alloy on the surface of a zirconium alloy substrate to obtain a FeCrAl composite coating; wherein the flow rate of the powder feeding gas used in the ultra-high-speed laser cladding technology is 14-15 L / min, the laser power is 250-300 W, the laser moving speed is 5-7 m / min, the cladding line speed is 20-40 m / min, the powder feeding amount is 3.9250 g / min, the single-pass lateral displacement is 0.6-0.8 mm, and the distance between the laser head and the zirconium alloy substrate is 17.5-19 mm.

[0055] Furthermore, the powder feeding gas includes an inert gas, such as argon.

[0056] In some preferred embodiments, the preparation method further comprises: before the cladding treatment, grinding and cleaning the zirconium alloy substrate; wherein the cleaning treatment comprises: using ethanol or acetone to clean the surface of the zirconium alloy substrate obtained by the grinding treatment, at least for removing grease.

[0057] The present invention adopts a method of preheating the substrate, holding a butane gas spray gun, rotating a machine tool fixture, and uniformly heating the substrate alloy tube at 200-500° C. to reduce the possibility of crack formation in the coating and reduce the size of unmelted particles.

[0058] The embodiment of the present invention provides a method for preparing a FeCrAl composite coating. 4 Under the conditions of high cooling rate of 10000K / s and high overlap rate of 60% to 90%, the coating structure is regulated, the coating structure is uniform and fine, the anti-oxidation performance is improved, and the performance "pollution" of the coating caused by the substrate components is effectively avoided, that is, the dilution rate is low, and due to its metallurgical bonding characteristics, the coating has high bonding strength. The preparation method of the present invention includes the following steps:

[0059] a. Pretreatment of the matrix material: The Zr-4 alloy tube is polished with sandpaper of different mesh sizes; then, it is ultrasonically cleaned with alcohol and acetone for 20 minutes; after cleaning, it is placed in a drying oven for drying;

[0060] b. Matrix installation: clamp the Zr-4 alloy tube in the fixture of the ultra-high-speed laser cladding machine, and the length of the zirconium alloy tube is 300 mm;

[0061] c. Preheating the substrate: Rotate the machine tool fixture and use a butane gas spray gun to evenly heat the Zr-4 alloy tube until the tube is red;

[0062] d. Cladding coating: The defocus amount in the ultra-high-speed laser cladding equipment is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by using a powder feeding gas; wherein the flow rate of the powder feeder gas used in the cladding technology is 14 L / min, the laser power is 250-300 W, the cladding line speed is 20-40 m / min, the powder feeder disk speed is 10%, and the single-pass traverse is 0.6-0.8 mm, and the FeCrA composite 1 coating is obtained, and the cladding is stopped and naturally cooled to room temperature.

[0063] Furthermore, the powder feeding gas is argon.

[0064] Furthermore, the purity of the FeCrAl powder is above 99.9%.

[0065] Furthermore, during the cladding process, the fixture maintains a high-speed rotation of 20 to 40 m / min, and the laser movement speed is 5 to 7 m / min; an ultra-high-speed laser cladding process is used to clad the coating.

[0066] Furthermore, at a laser power of 250 W, the coating prepared by cladding has a uniform structure, fine grains, and almost no cracks, which can easily and well protect the substrate from high-temperature water vapor corrosion.

[0067] The FeCrAl composite coating of the present invention can form a metallurgical bond with the substrate, and the coating structure is uniform and fine, which can reduce the reaction rate of the cladding material with water vapor at high temperature, delay the core degradation process, and has an excellent bonding force of 90N, and the coating strength is as high as 800Hv 0.05 , which makes the zirconium alloy tube have better high temperature oxidation resistance and good mechanical properties.

[0068] Another aspect of the embodiments of the present invention further provides the use of the aforementioned FeCrAl composite coating in the protection of curved surface parts.

[0069] Another aspect of an embodiment of the present invention further provides a fuel cladding device, which includes a zirconium alloy tube and a FeCrAl composite coating prepared by the aforementioned preparation method.

[0070] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0071] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0072] In the present invention, in order to ensure that the oxidation weight gain data is authentic and reliable, the sample is weighed three times before and after each oxidation, and the average value is taken as the final data.

[0073] Example 1

[0074] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0075] b. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0076] c. Preheating the substrate: Rotate the machine tool fixture, hold a butane gas spray gun, and evenly heat the Zr-4 alloy tube at 400°C until the tube body turns red;

[0077] d. Cladding coating: The ultra-high-speed laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 15 s. In this process, the FeCrAl powder in the powder feeding tube is stirred into the powder feeding plate, and the powder discharge state is checked. High-purity argon gas (argon purity> 99.9%) is used to blow the FeCrAl powder into the melting zone on the surface of the substrate; wherein, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology is 14 L / min, the laser power is 250 W, the cladding line speed is 40 m / min, the powder feeder plate speed is 10%, and the single-pass traverse is 0.6 mm. The FeCrAl composite coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0078] e. Structure and composition test: such as Figure 1a-1b As shown, the coating is metallurgically bonded to the Zr-4 alloy tube, the coating structure is uniform and fine, the thickness of the dilution layer is 20 to 40 μm, and there are no unmelted powder particles. Figure 2 It is the coating grain distribution and size diagram. The grain size is between 10 and 30 μm. Figure 3The X-ray diffraction pattern shows that the main phase of the FeCrAl composite coating is a Fe-Cr solid solution with a body-centered cubic structure.

[0079] f. Mechanical properties test:

[0080] The Revetest scratch test system was used to measure the bonding strength between the coating and the substrate. The applied load pressure was 150N. The scratches on the coating surface were as follows: Figure 4 As shown in the figure, the coating is completely broken at about 90 N, so the coating bonding force is about 90 N. The surface roughness of the coating is measured using a VK-X1000 laser confocal microscope, as shown in the figure. Figure 5a-Figure 5b As shown, the surface roughness of the coating prepared by ultra-high-speed laser cladding is Ra=6.5μm, and the surface roughness of the coating prepared by traditional laser cladding is Ra=44.1μm. The roughness of the coating prepared by ultra-high-speed laser cladding technology is reduced by 37.6μm, which greatly reduces the surface roughness of the coating. The HV1000IS microhardness tester is used to measure the microhardness of the coating, and the loading load and time are set to 0.05kg and 10s respectively. In order to ensure the accuracy and representativeness of the data, 10 test points are selected each time the sample is measured, and then the average value of the 10 points is calculated as the final data of the microhardness of the coating. As shown Fig.18 As shown, the hardness of the ultra-high-speed laser cladding coating is about 800Hv 0.05 , while the hardness of traditional laser cladding coating is about 450Hv 0.05 , hardness increased by 78%.

[0081] g. Antioxidation performance test: A high-temperature isothermal steam test system (consisting of a peristaltic pump, a steam generator, a flow meter, and a BTF-1400C series tubular furnace) was used to test the high-temperature steam oxidation performance of the prepared coating under a simulated LOCA environment. The sample was weighed before oxidation, and the insulation temperature was set to 1200°C. The insulation time was 10, 30, 45, 60, and 120 minutes. After oxidation, the sample was cooled to room temperature in the furnace and weighed. The oxidation weight gain curve of the sample was obtained by Figure 6 As shown, it can be seen that the sample growth curve from 0 to 120 min is stable. Figure 7 The cross-sectional SEM and EDS images of the FeCrAl composite coating after oxidation in high-temperature water vapor at 1200°C for 60 minutes show that the coating structure is intact. Figure 8 This is the X-ray diffraction pattern of the surface after oxidation. CrO2 and Al2O3 oxide films are formed on the coating surface to protect the substrate, indicating that the coating can effectively protect the substrate from corrosion in a high-temperature water vapor environment of 1200℃ for 60 minutes.

[0082] Example 2

[0083] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0084] b. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0085] c. Preheating the substrate: Rotate the machine tool fixture, hold a butane gas spray gun, and evenly heat the Zr-4 alloy tube at 400°C until the tube body turns red;

[0086] d. Cladding coating: The ultra-high-speed laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 15 s. In this process, the FeCrAl powder in the powder feeding tube is waited for to be fed into the powder feeding plate, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by high-purity argon gas (argon purity>99.9%); wherein, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology is 14 L / min, the laser power is 275 W, the cladding line speed is 40 m / min, the powder feeder plate speed is 10%, and the single-pass traverse is 0.6 mm, and the FeCrAl composite coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0087] Example 3

[0088] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0089] b. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0090] c. Preheating the substrate: Rotate the machine tool fixture, hold a butane gas spray gun, and evenly heat the Zr-4 alloy tube at 400°C until the tube body turns red;

[0091] d. Cladding coating: The ultra-high-speed laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 15 s. In this process, the FeCrAl powder in the powder feeding tube is waited for to be fed into the powder feeding plate, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by high-purity argon gas (argon purity>99.9%); wherein, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology is 14 L / min, the laser power is 300 W, the cladding line speed is 40 m / min, the powder feeder plate speed is 10%, and the single-pass traverse is 0.6 mm, and the FeCrAl composite coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0092] Comparative Example 1

[0093] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0094] b. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0095] c. Cladding coating: The ultra-high-speed laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 15 s. In this process, the FeCrAl powder in the powder feeding tube is waited for to be fed into the powder feeding plate, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by high-purity argon (argon purity> 99.9%). Among them, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology is 14 L / min, the laser power is 275 W, the cladding line speed is 40 m / min, the powder feeder plate speed is 10%, and the single-pass traverse is 0.8 mm. The FeCrAl coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0096] d. Structure and composition test: The coating is metallurgically bonded to the substrate. The SEM image of the coating cross section is as follows: Fig.11 As shown, the coating thickness is 15N20μm, the coating is thin, the coating has crack defects and the unmelted powder particles are large.

[0097] e. Anti-oxidation performance test: The high-temperature isothermal steam test system was used to test the high-temperature water vapor oxidation performance of the prepared coating in a simulated LOCA environment. The sample was weighed before oxidation, and the insulation temperature was set to 1200°C for 60 minutes. After oxidation, the sample was cooled to room temperature in the furnace and weighed. The oxidation weight gain was 3.183251 mg / cm 2, and the sample obtained by cladding after preheating the substrate (weight gain is 3.017462mg / cm 2 ) compared to the sample, the weight gain is significantly greater. The cross section of the sample after corrosion is as follows Fig.12 As shown, there are a large number of holes in the substrate. Not only does the coating fail to provide protection, but the substrate also fails due to crack initiation.

[0098] Comparative Example 2

[0099] Due to the working characteristics of traditional laser cladding, coating cannot be clad on the pipe, so Zr-4 alloy plate is used for traditional laser cladding.

[0100] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy plate with a size of 10×15mm, and polish the zirconium alloy matrix material with 100#, 200#, 400#, and 800# sandpaper in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0101] b. Preheating of substrate installation: Place the Zr-4 alloy plate after the above treatment on the heating table, set the heating table to 300°C, and focus the laser red dot on the starting point of cladding on the sample;

[0102] c. Cladding coating: the laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 20 s. In this process, the FeCrAl powder in the powder feeding tube is waited for to be fed into the powder feeding plate, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by high-purity argon gas (argon purity> 99.9%); wherein, the flow rate of the powder feeder gas used in the cladding technology is 15 L / min, the laser power is 300 W, the laser rate is 8 mm / s, the return rate is 15 mm / s, the powder feeder plate speed is 5%, the single-pass traverse is 1 mm, and the single-pass length is 25 mm. The FeCrAl coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0103] d. Structure and composition test: The coating is metallurgically bonded to the substrate. The SEM image of the coating cross section is as follows: Fig.13a * Fig.13b As shown, the coating thickness is about 1 mm, and there is an obvious dilution layer with a thickness of 140 to 370 μm.

[0104] e. Anti-oxidation performance test: The high-temperature isothermal steam test system was used to test the high-temperature water vapor oxidation performance of the prepared coating in a simulated LOCA environment. The sample was weighed before oxidation, the insulation temperature was set to 1200°C, and the insulation time was 60 minutes. After oxidation, the sample was cooled to room temperature in the furnace and weighed. The sample weight gain was 9.451597 mg / cm 2, and the sample made by ultra-high-speed laser cladding (weight gain is 2.722357428mg / cm 2 ) compared to the original sample, the weight gain is large. The cross section of the sample after corrosion is as follows Fig.14 As shown, the coating is mixed with a large amount of Zr elements from the substrate tube, which dilutes the composition of the FeCrAl coating, causing changes in the alloy composition and relative content of elements in the FeCrAl coating, changing the phase structure of the FeCrAl alloy composition, and destroying the high-temperature steam oxidation resistance mechanism of the FeCrAl alloy, thereby reducing the high-temperature oxidation resistance of the FeCrAl coating.

[0105] Comparative Example 3

[0106] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0107] b. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0108] c. Preheating the substrate: Rotate the machine tool fixture, hold a butane gas spray gun, and evenly heat the Zr-4 alloy tube at 400°C until the tube body turns red;

[0109] d. Cladding coating: The ultra-high-speed laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 15 s. In this process, the FeCrAl powder in the powder feeding tube is waited for to be fed into the powder feeding plate, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by high-purity argon gas (argon purity>99.9%); wherein, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology is 14 L / min, the laser power is 200 W, the cladding linear speed is 40 m / min, the powder feeder plate speed is 10%, and the single-pass traverse is 0.6 mm. The FeCrAl coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0110] e. Structure and composition test: SEM image of coating cross section as shown below: Fig.15 As shown, this process has low power consumption, the unmelted powder particles are large, and the coating cannot be completely layered.

[0111] Comparative Example 4

[0112] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0113] b. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0114] c. Preheating the substrate: Rotate the machine tool fixture, hold a butane gas spray gun, and evenly heat the Zr-4 alloy tube at 400°C until the tube body turns red;

[0115] d. Cladding coating: The ultra-high-speed laser cladding defocus amount is set to +0 mm, that is, the working distance of the cladding head is 20.6 mm, and the waiting time is set to 15 s. In this process, the FeCrAl powder in the powder feeding tube is waited for to be fed into the powder feeding plate, and the FeCrAl powder is blown into the melting zone on the surface of the substrate by high-purity argon gas (argon purity>99.9%); wherein, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology is 14 L / min, the laser power is 400 W, the cladding linear speed is 40 m / min, the powder feeder plate speed is 10%, and the single-pass traverse is 0.6 mm. The FeCrAl coating is obtained, the cladding is stopped, and the sample is taken out after natural cooling to room temperature.

[0116] e. Structure and composition test: The coating surface is as follows: Fig.16 As shown, the coating cladding is uneven in a single pass, with obvious shrinkage, and the power is too large, resulting in structural changes.

[0117] Comparative Example 5

[0118] a. Pretreatment of the matrix material: First, prepare a Zr-4 alloy tube with an outer diameter of 9.5 mm, an inner diameter of 8.36 mm, and a length of 300 mm. Use 100#, 200#, 400#, and 800# sandpaper to polish the zirconium alloy matrix material in sequence; then use alcohol and acetone to ultrasonically clean it for 20 minutes; after cleaning, put it in a drying oven to dry;

[0119] b. Preparation of coating materials: Use a precision balance to weigh 100g of coating powders of four different element ratios. The coating element ratios are shown in Table 1:

[0120] Table 1 Composition of FeCrAl powders with different element ratios

[0121]

[0122] c. Installation of substrate: clamp the Zr-4 alloy tube after the above treatment in the fixture of the ultra-high-speed laser cladding machine tool, and keep its rotation process stable;

[0123] d. Preheating the substrate: Rotate the machine tool fixture, hold the butane gas spray gun, and evenly heat the Zr-4 alloy tube at 400°C until the tube body turns red;

[0124] e. Cladding coating: The ultra-high-speed laser cladding defocus amount was set to +0 mm, that is, the working distance of the cladding head was 20.6 mm, and the waiting time was set to 15 s. In this process, the FeCrAl powder in the powder feeding tube was waited for to be fed into the powder feeding plate, and high-purity argon gas (argon purity> 99.9%) was used to blow the FeCrAl powder into the melting zone on the surface of the substrate; wherein, the flow rate of the powder feeder gas used in the ultra-high-speed cladding technology was 14 L / min, the laser power was 250 W, the cladding line speed was 40 m / min, the powder feeder plate speed was 10%, and the single-pass traverse was 0.6 mm, and four types of FeCrAl coatings were obtained, and the cladding was stopped. The samples were taken out after natural cooling to room temperature.

[0125] f. Coating performance test: A high-temperature isothermal steam test system (consisting of a peristaltic pump, a steam generator, a flow meter, and a BTF-1400C series tubular furnace) was used to test the high-temperature steam oxidation performance of the prepared coating under a simulated LOCA environment. The sample was weighed before oxidation, and the insulation temperature was set to 1200°C. The insulation time was 10, 30, 45, 60, and 120 minutes. After oxidation, the sample was cooled to room temperature in the furnace and weighed. The oxidation weight gain curve of the sample was obtained by Fig.17 As shown in the figure, it can be seen that the coating with a powder element ratio of 68wt% Fe, 25wt% Cr, and 7wt% Al has the lowest oxidation weight gain and the best water vapor oxidation resistance. The microhardness of the coating is measured using a HV1000IS microhardness tester. Fig.18 It can be seen that the coating with a powder element ratio of 68wt% Fe, 25wt% Cr, and 7wt% Al has the highest hardness.

[0126] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0127] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A FeCrAl composite coating for a zirconium alloy surface, characterized in that: The FeCrAl composite coating comprises a metallurgical bonding layer and a FeCrAl cladding layer which are sequentially formed on the surface of a substrate. The FeCrAl composite coating is formed by cladding FeCrAl alloy on the surface of a zirconium alloy substrate using ultra-high-speed laser cladding technology. In the direction away from the substrate surface, the contents of Fe, Cr and Al elements in the metallurgical bonding layer gradually increase. The metallurgical bonding layer is mainly composed of Fe-Zr solid solution and Cr-Zr solid solution. The main phase of the FeCrAl cladding layer includes an α-Fe-based solid solution alloy with a body-centered cubic structure. The grain size of the FeCrAl cladding layer is 10 to 30 μm.

2. The FeCrAl composite coating according to claim 1, characterized in that: The FeCrAl cladding layer comprises the following components calculated by mass percentage: 68wt% Fe, 25wt% Cr and 7wt% Al; and / or, the thickness of the metallurgical bonding layer is 0 to 60 μm; And / or, the FeCrAl cladding layer has a thickness of 20-50 μm.

3. The FeCrAl composite coating according to claim 1, characterized in that: The α-Fe based solid solution alloy includes Fe—Cr solid solution; preferably, the content of Fe—Cr solid solution in the FeCrAl coating is 74-88wt%.

4. The FeCrAl composite coating according to claim 1, characterized in that: The zirconium alloy substrate comprises a Zr-4 alloy tube; preferably, the length of the Zr-4 alloy tube is 300 to 400 mm.

5. The method for preparing a FeCrAl composite coating on a zirconium alloy surface according to any one of claims 1 to 4, characterized in that: include: Providing a zirconium alloy substrate; Preheating the zirconium alloy substrate to 200-500° C.; Furthermore, the FeCrAl alloy is clad on the surface of a zirconium alloy substrate using an ultra-high-speed laser cladding technology to obtain a FeCrAl composite coating on the surface of the zirconium alloy.

6. The preparation method according to claim 5, characterized in that: The average particle size of the FeCrAl alloy is 10 to 30 μm; and / or, the purity of the FeCrAl alloy is above 99.9wt%; And / or, the FeCrAl alloy includes the following components calculated by mass percentage: 68 wt % Fe, 25 wt % Cr and 7 wt % Al.

7. The preparation method according to claim 5, characterized in that: Specifically include: The FeCrAl alloy is clad on the surface of the zirconium alloy substrate by ultra-high-speed laser cladding technology to obtain a FeCrAl composite coating; wherein the flow rate of the powder feeding gas used in the ultra-high-speed laser cladding technology is 14-15 L / min, the laser power is 250-300 W, the laser moving speed is 5-7 m / min, the cladding line speed is 20-40 m / min, the powder feeding amount is 3.9250 g / min, the single-pass lateral movement is 0.6-0.8 mm, and the distance between the laser head and the zirconium alloy substrate is 17.5-19 mm; preferably, the powder feeding gas includes an inert gas.

8. The preparation method according to claim 5, characterized in that: Also includes: Before the cladding treatment, the zirconium alloy substrate is first polished and cleaned; wherein the cleaning treatment includes: using ethanol or acetone to clean the surface of the zirconium alloy substrate obtained by the polishing treatment, at least for removing grease.

9. Use of the FeCrAl composite coating according to any one of claims 5 to 8 in the protection of curved surface parts.

10. A fuel cladding device, characterized in that: The invention comprises a zirconium alloy tube and a FeCrAl composite coating prepared by the preparation method described in any one of claims 5 to 8.

Citation Information

Patent Citations

  • Preparation method for nuclear zirconium alloy coating

    CN110835755A

  • Preparation method for superspeed laser cladding of AlCrFeNiCu high-entropy alloy coating on surface of zirconium rod

    CN117344303A

  • Cr gradient composite coating for fuel cladding surface as well as preparation method and application of Cr gradient composite coating

    CN117535660A

  • Accident-resistant zirconium alloy cladding surface composite coating and preparation method thereof

    CN117737652A

Cited By

  • Cr-Si alloy coating for zirconium alloy surface as well as preparation method and application of Cr-Si alloy coating

    CN121674961A