Method for producing lithium and alkali metal salt through molten salt electrolysis of lithium ore

The molten salt electrolysis method is used to enrich lithium and alkali metal salts in lithium ores, which solves the problems of environmental pollution and low recovery rate caused by the sulfuric acid method, achieves efficient recovery of lithium and alkali metal salts, and reduces production costs and environmental pollution. .

CN118773671APending Publication Date: 2024-10-15FUJIAN BAOXIONG IND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410917899.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Among the existing lithium ore processing technologies, the sulfuric acid method causes high-aluminum-silicon leaching slag to cause serious harm to the environment. The metal recovery rate is low and the cost is high. The electrothermal method has high equipment requirements, high reaction temperature, large amount of smoke and dust, poor recovery rate, and is difficult to process. control.

Method used

Using molten salt electrolysis method, the fluoride salt in lithium ore is used as the electrolyte, and the electrochemical reaction is carried out through the carbon block or inert metal anode and liquid aluminum cathode in the electrolytic cell to generate lithium fluoride and alkali metal salts, silicon-aluminum alloy Liquid precipitation and separation enriches lithium and alkali metal salts, reduces slag generation, and improves recovery rate.

Benefits of technology

It achieves efficient enrichment of lithium and alkali metal salts, increases the metal recovery rate, produces no slag, is environmentally friendly, reduces production costs, and solves the problems of high costs, low recovery rates, and large pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773671A_ABST
    Figure CN118773671A_ABST
Patent Text Reader

Abstract

According to the method for producing the lithium and the alkali metal salt through the molten salt electrolysis of the lithium ore, lithium and the alkali metal salt are enriched in the electrolyte through the molten salt electrolysis of the lithium ore, elements such as silicon and aluminum are separated out at the cathode, lithium and the alkali metal salt are enriched in the electrolyte, lithium, sodium, potassium, fluorine, silicon and aluminum in lithium ore gangue are comprehensively utilized, and the lithium and the alkali metal salt are recycled. The method has the advantages of high metal recovery rate, no generation of slag, environmental friendliness due to recovery of fluorine in ore, reduction of environmental pollution, low requirements on production conditions, high lithium content in enriched lithium and alkali metal salt, provision of conditions for subsequent efficient production of lithium, alkali metal and salt, reduction of the production cost of lithium, alkali metal and salt, and realization of industrial production. The problems that an existing lithium, alkali metal and salt technology is high in cost, low in metal recovery rate and large in pollution, and leaching residues are difficult to treat are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ore processing, and in particular to a method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore. Background Art

[0002] Lithium is an important strategic resource. With the rapid development of new energy vehicles, lithium is widely used as the positive electrode material of high energy density lithium-ion batteries.

[0003] At present, the production technology of lithium carbonate generally adopts sulfuric acid acidification roasting method, that is, spodumene is used as raw material, and it is produced through calcination transformation, acidification roasting, leaching, purification, lithium precipitation and other processes. However, for every ton of lithium salt produced, dozens of tons of high-aluminum silicon leaching slag will be produced, causing serious harm to the environment. Therefore, it is crucial to invent a green, environmentally friendly, resource-based comprehensive utilization of lithium ore to produce lithium carbonate.

[0004] The invention patent with application number 201080065025.X discloses a method for manufacturing lithium carbonate, which includes: calcining α spodumene ore to generate β spodumene; then ball milling after cooling, mixing with sulfuric acid, transferring to a sulfation kiln, and sulfating the β spodumene at high temperature; leaching the sulfated β spodumene with water to generate a lithium sulfate solution; and then through a series of purification and impurity removal measures, finally obtaining lithium carbonate and sodium sulfate.

[0005] The invention patent with application number 201110000790.X discloses a method for producing lithium carbonate and lithium hydroxide. The spodumene concentrate is roasted at a high temperature of 1050-1100°C, cooled, finely ground, and 98% concentrated sulfuric acid is added. After acidification and roasting at 250-300°C, it is subjected to wet extraction to remove calcium and magnesium impurities. After evaporation and concentration, and filter pressing, a lithium sulfate solution is obtained to obtain lithium carbonate; lithium hydroxide can also be obtained by adding barium hydroxide to the lithium carbonate mother liquor.

[0006] The invention patent with application number CN202111103686.3 discloses a method for producing silicon-manganese alloy from lithium ore and enriching lithium. Lithium ore, carbonaceous reducing agent and manganese ore are mixed in a certain proportion and put into a closed submerged arc furnace. A protective atmosphere is introduced, and the temperature of the submerged arc furnace is raised to 1000°C. The smelting is carried out for 24 hours, so that the clay-type lithium ore in the material undergoes a carbon thermal reduction reaction with anthracite with the participation of pyrolusite. After the smelting is completed, lithium-rich ash is recovered in the smoke system of the submerged arc furnace, manganese-silicon alloy is obtained at the iron outlet, and alumina-rich slag is obtained at the slag outlet.

[0007] The invention patent with application number CN110195159A discloses a method for preparing silicon-aluminum alloy and enriching lithium from lithium ore. Lignite and spodumene are mixed at a molar ratio of 6 to 7:1 between C in lignite and spodumene, and clay is added and mixed evenly. The mixture is pressed into shape and then calcined in an electric arc furnace at a temperature controlled at 2000 to 2100°C. The calcined volatiles are collected to obtain lithium-rich ash, and the calcined products are condensed to obtain aluminum-silicon alloy.

[0008] The above method of extracting lithium from lithium ore using sulfuric acid method obtains lithium in the form of lithium salts such as lithium carbonate and lithium hydroxide, and the main elements of lithium ore, aluminum and silicon, enter the slag after filtration. A large amount of leached slag contains sulfate and alkali metal salts that are difficult to digest, causing serious problems to the environment, low metal recovery rate, high cost, and the electric heating method has high requirements on equipment, high reaction temperature, large amount of smoke, poor recovery rate, and difficult to control cost. Summary of the invention

[0009] 1. Technical issues to be resolved

[0010] In order to solve the above problems in the prior art, the present invention provides a method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore.

[0011] (II) Technical solution

[0012] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0013] A method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore, comprising the following steps:

[0014] S1: Using lithium ore as electrolysis raw material and using fluoride salt contained in the ore as electrolyte; feeding lithium ore and fluoride salt into the electrolytic cell;

[0015] S2: The anode in the electrolytic cell is a carbon block or an inert metal anode, and the cathode in the electrolytic cell is liquid aluminum;

[0016] S3: The electrolytic cell is powered on, and lithium ore is continuously added to the molten electrolyte. Electrochemical reactions occur at the two electrodes, and CO, CO2 or O2 gas is generated at the anode. Liquid silicon-aluminum alloy liquid is precipitated at the cathode, and the liquid silicon-aluminum alloy liquid is deposited at the bottom of the tank. It is regularly removed for refining, and part of the metallic aluminum is recycled as cathode liquid aluminum. The lithium and alkali metal compounds contained in the lithium ore react with the fluoride in the electrolyte to generate lithium fluoride and alkali metal salts. With the continuous addition of lithium ore, lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts are enriched in the electrolyte.

[0017] S4: Collecting electrolytes containing lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts, adding new electrolytes, and separating and treating electrolytes enriched with lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts to obtain lithium, sodium, potassium, rubidium and cesium salts.

[0018] Preferably, the ore is one or more of spodumene, lepidolite or clay-type lithium ore, and the lithium ore is calcined at 300-800° C. to remove moisture, and the particle size is less than 100 mesh.

[0019] Preferably, the temperature of the electrolysis reaction in step S2 is controlled between 700 and 1100° C., the cell voltage is 3.0 to 6.0 V, and the electrolyte is lithium-rich and / or alkali metal salt.

[0020] (III) Beneficial effects

[0021] The beneficial effects of the present invention are as follows: by adopting the above technical scheme, lithium ore molten salt electrolysis is used to enrich lithium and alkali metal salts in the electrolyte, silicon, aluminum and other elements are precipitated and separated at the cathode, lithium and alkali metal salts are enriched in the electrolyte, lithium, sodium, potassium, fluorine, silicon and aluminum in the lithium ore vein are comprehensively utilized, the metal recovery rate is high, no slag is generated and the fluorine in the ore is recovered, which is more environmentally friendly and reduces environmental pollution, the production conditions are not demanding, the lithium content in the enriched lithium and alkali metal salts is high, conditions are provided for the subsequent efficient production of lithium and alkali metals and salts, the production cost of lithium and alkali metals and salts is reduced, and the problems of high process cost of lithium and alkali metals and salts, low metal recovery rate, high pollution and difficult treatment of leached slag are solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of electrolysis in an electrolytic cell in a method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore. DETAILED DESCRIPTION

[0023] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0024] Please refer to Figure 1 , the first embodiment of the present invention:

[0025] A method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore, comprising the following steps:

[0026] S1: Using lithium ore as electrolysis raw material and using fluoride salt contained in the ore as electrolyte; feeding lithium ore and fluoride salt into the electrolytic cell;

[0027] S2: The anode in the electrolytic cell is a carbon block or an inert metal anode, and the cathode in the electrolytic cell is liquid aluminum;

[0028] S3: The electrolytic cell is powered on, and lithium ore is continuously added to the molten electrolyte. Electrochemical reactions occur at the two electrodes, and CO, CO2 or O2 gas is generated at the anode. Liquid silicon-aluminum alloy liquid is precipitated at the cathode, and the liquid silicon-aluminum alloy liquid is deposited at the bottom of the tank. It is regularly removed for refining, and part of the metallic aluminum is recycled as cathode liquid aluminum. The lithium and alkali metal compounds contained in the lithium ore react with the fluoride in the electrolyte to generate lithium fluoride and alkali metal salts. With the continuous addition of lithium ore, lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts are enriched in the electrolyte.

[0029] S4: Collecting electrolytes containing lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts, adding new electrolytes, and separating and treating electrolytes enriched with lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts to obtain lithium, sodium, potassium, rubidium and cesium salts.

[0030] In this embodiment, the ore is one or more of spodumene, lepidolite or clay-type lithium ore, and the lithium ore is calcined at 300-800° C. to remove moisture, and the particle size is less than 100 mesh.

[0031] In this embodiment, the temperature of the electrolysis reaction in step S2 is controlled between 700 and 1100° C., the cell voltage is 3.0 to 6.0 V, and the electrolyte is lithium-rich and / or alkali metal salt;

[0032] See also Figure 1 , a method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore, the specific steps are as follows:

[0033] (1) Spodumene is used as the electrolyte raw material, the powder particle size is controlled to be less than 100 mesh, and the powder is calcined at 400° C. to remove moisture, and 1000 g of Na3AlF6-AlF3 cryolite-based molten salt is used as the first electrolyte, and the mixture is respectively fed into the electrolytic cell; the first addition amount of spodumene is 5% of the total mass of the cryolite-based molten salt and spodumene;

[0034] The specific composition is: The analysis of spodumene is shown in the table below, and the molecular ratio of sodium fluoride to aluminum fluoride is 2.0;

[0035]

[0036] (2) The anode carbon blocks required for electrolysis are used in the anode assembly section together with the guide rods to form an anode group; the cathode is liquid aluminum;

[0037] (3) After the electrolytic cell is powered by direct current, lithium ore is continuously added to the molten electrolyte, and an electrochemical reaction occurs at the two electrodes. CO2, CO, and O2 gases are generated at the anode. Spodumene is added every half an hour, and the amount of spodumene added each time is 60% of the amount of spodumene added for the first time. No cryolite is needed to be added subsequently. The electrolysis is continued for 24 hours, and liquid silicon-aluminum alloy is precipitated on the cathode and deposited at the bottom of the tank. It is removed regularly, and the electrolyte volatiles are captured and reused, and the remaining electrolyte components are detected. Lithium fluoride and alkali metal salt electrolytes are separated and treated to obtain lithium, sodium, potassium, rubidium, and cesium.

[0038] Electrolysis parameters: temperature controlled at 970°C, cell voltage 3.95V.

[0039] The composition of lithium-rich alkali metal electrolytes is shown in the table below;

[0040] Element Li Na Al K F Si content% 11.07 17.63 1.51 1.71 47.11 1.78

[0041] (4) Lithium and alkali metal salts can be obtained by treating lithium-rich electrolytes according to the current mature process.

[0042] Example 2

[0043] A method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore, the specific steps are as follows:

[0044] (1) Using lepidolite as electrolyte raw material, the powder particle size is controlled between 100 and 200 meshes, calcined at 500° C. to remove moisture, and 1000 g of Na3AlF6-AlF3 cryolite-based molten salt is used as the first electrolyte, and then fed into the electrolytic cell respectively; the first addition amount of lepidolite is 6% of the total mass of cryolite-based molten salt and lepidolite;

[0045] The specific composition is: the composition of lepidolite is shown in the table below, the molecular ratio of cryolite-based molten salt, that is, the molecular ratio of sodium fluoride to aluminum fluoride is 2.3;

[0046]

[0047] (2) The anode carbon blocks required for electrolysis are used in the anode assembly section together with the guide rods to form an anode group; the cathode is liquid aluminum;

[0048] (3) After the electrolytic cell is supplied with direct current, lithium mica is continuously added to the molten electrolyte, and an electrochemical reaction occurs at the two electrodes. CO2, CO, and O2 gases are generated at the anode. The lithium mica is replenished every half an hour, and the amount of lithium mica added each time is 40% of the mass of the lithium mica added for the first time. No cryolite is required to be added subsequently. The electrolysis is continued for 48 hours, and liquid silicon-aluminum alloy is precipitated on the cathode and deposited at the bottom of the tank. It is removed regularly, and the electrolyte volatiles are captured and reused, and the remaining electrolyte components are detected; lithium fluoride and alkali metal salt electrolytes are separated and treated to obtain lithium, sodium, potassium, rubidium, and cesium.

[0049] Electrolysis parameters: temperature controlled at 975°C, cell voltage 4.05V.

[0050] The composition of lithium-rich electrolyte is shown in the table below;

[0051] Element Li Na Al K F Si content% 5.89 15.59 1.84 20.74 41.35 1.12

[0052] (4) Lithium and alkali metal salts can be obtained by treating lithium-rich electrolytes according to the current mature process.

[0053] Example 3

[0054] A method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore, the specific steps are as follows:

[0055] (1) Using lepidolite as electrolyte raw material, the powder particle size is controlled between 100 and 300 meshes, calcined at 450° C. to remove moisture, and 1000 g of Na3AlF6-AlF3 cryolite-based molten salt is used as the first electrolyte, and the mixture is respectively fed into an electrolytic cell; the first addition amount of lepidolite is 7% of the total mass of the cryolite-based molten salt and lepidolite;

[0056] The specific composition is: the composition of lepidolite is shown in the table below; the molecular ratio of cryolite-based molten salt, that is, the molecular ratio of sodium fluoride to aluminum fluoride is 2.0;

[0057]

[0058] (2) The anode carbon blocks required for electrolysis are used in the anode assembly section together with the guide rods to form an anode group; the cathode is liquid aluminum;

[0059] (3) After the electrolytic cell is supplied with direct current, lithium mica is continuously added to the molten electrolyte, and an electrochemical reaction occurs at the two electrodes. CO2, CO, and O2 gases are generated at the anode. The lithium mica is replenished every half an hour, and the amount of lithium mica added each time is 50% of the mass of the lithium mica added for the first time. No cryolite is required to be added subsequently. The electrolysis is continued for 36 hours, and liquid silicon-aluminum alloy is precipitated on the cathode and deposited at the bottom of the tank. It is removed regularly, and the electrolyte volatiles are captured and reused, and the remaining electrolyte components are detected; lithium fluoride and alkali metal salt electrolytes are separated and treated to obtain alkali metals and salts such as lithium, sodium, potassium, rubidium, and cesium.

[0060] Electrolysis parameters: temperature controlled at 960°C, cell voltage 4.05V.

[0061] The composition of lithium-rich electrolyte is shown in the table below;

[0062] Element Li Na Al K F Si content% 8.32 13.38 1.41 18.84 42.47 1.02

[0063] (4) Lithium and alkali metal salts can be obtained by treating lithium-rich electrolytes according to the current mature process.

[0064] From the above examples, it can be seen that adding lithium ore to cryolite molten salt is beneficial to the electrolysis of aluminum silicon, and at the same time, alkali metal salts such as lithium are enriched in the electrolyte. The higher the lithium content in the lithium ore, the higher the lithium content enriched in the electrolyte; the optimal molecular ratio of NaF and AlF3 in cryolite molten salt is controlled at 2 to 2.5. The optimal electrolysis temperature is controlled between 960℃ and 980℃; according to the different lithium content in the raw materials, the initial addition amount of lithium ore is adjusted, and the initial addition amount of lithium ore ranges from 5% to 7% of the total mass of cryolite-based molten salt and lithium ore.

[0065] The main reaction process involved in the present invention is as follows:

[0066] Aluminum:

[0067]

[0068] 4A l+3S i O2→2A l2O3+3S i

[0069] Silicon:

[0070] S i 4+ +4e-→S i

[0071] Lithium:

[0072] 3L i2O+2A l F3→6L i F+A l2O3

[0073] The present invention adopts lithium ore molten salt electrolysis to enrich lithium and alkali metal salts in the electrolyte, silicon and aluminum elements are precipitated and separated at the cathode, lithium and alkali metal salts are enriched in the electrolyte, and the enriched lithium and alkali metal salts can promote the electrolysis of aluminum silicon on the one hand, and are beneficial to the subsequent production of lithium and alkali metal salts on the other hand.

[0074] Al2O3 and SiO2 in lithium ore have high solubility in aluminum fluoride-lithium fluoride-potassium fluoride melt and dissolve quickly. They can be evenly dispersed in the electrolyte and are quickly reduced to silicon by aluminum. Since the decomposition voltage of SiO2 is lower than that of Al2O3, silicon will be electrolytically precipitated first. Part of the silicon in the aluminum-silicon alloy is reduced and part is electrolytic.

[0075] In summary: lithium, sodium, potassium, fluorine, silicon and aluminum in lithium ore vein are all comprehensively utilized, with a high metal recovery rate, no slag is produced and the fluorine in the ore is recovered, which is more environmentally friendly and reduces environmental pollution. The production conditions are not demanding, and the enriched lithium and alkali metal salts have a high lithium content, which provides conditions for the subsequent efficient production of lithium and alkali metals and salts, reduces the production cost of lithium and alkali metals and salts, and solves the current problems of high process cost of lithium and alkali metals and salts, low metal recovery rate, high pollution, and difficult treatment of leaching slag.

[0076] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the specification and drawings of the present invention, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

[0077] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore, characterized in that: The following steps are included: S1: Using lithium ore as electrolysis raw material and using fluoride salt contained in the ore as electrolyte; feeding lithium ore and fluoride salt into the electrolytic cell; S2: The anode in the electrolytic cell is a carbon block or an inert metal anode, and the cathode in the electrolytic cell is liquid aluminum; S3: The electrolytic cell is powered on, and lithium ore is continuously added to the molten electrolyte. Electrochemical reactions occur at the two electrodes, and CO, CO2 or O2 gas is generated at the anode. Liquid silicon-aluminum alloy liquid is precipitated at the cathode, and the liquid silicon-aluminum alloy liquid is deposited at the bottom of the tank. It is regularly removed for refining, and part of the metallic aluminum is recycled as cathode liquid aluminum. The lithium and alkali metal compounds contained in the lithium ore react with the fluoride in the electrolyte to generate lithium fluoride and alkali metal salts. With the continuous addition of lithium ore, lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts are enriched in the electrolyte. S4: Collecting electrolytes containing lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts, adding new electrolytes, and separating and treating electrolytes enriched with lithium fluoride and sodium, potassium, rubidium and cesium alkali metal salts to obtain lithium, sodium, potassium, rubidium and cesium salts.

2. The method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore according to claim 1, characterized in that: The ore is one or more of spodumene, lepidolite or clay-type lithium ore, and the lithium ore is calcined at 300-800° C. to remove moisture, and the particle size is less than 100 meshes.

3. The method for producing lithium and alkali metal salts by molten salt electrolysis of lithium ore according to claim 1, characterized in that: In step S2, the temperature of the electrolysis reaction is controlled between 700 and 1100° C., the cell voltage is 3.0 to 6.0 V, and the electrolyte is lithium-rich and / or alkali metal salt.