Fog nickel electroplating process
Through the combined process of pre-plated nickel layer and phosphorus-containing base nickel layer, the problem of unstable consumption of matte nickel additives is solved, and a matte nickel coating with matte nickel and good ductility is achieved, which reduces production costs and maintenance frequency, and improves efficiency. Plating efficiency and controllability.
Patent Information
- Application Number
- CN202411013503.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing matte nickel electroplating technology, the consumption of matte nickel additives is unstable, which affects the appearance and quality of the coating, and requires frequent maintenance, which reduces the efficiency and controllability of electroplating.
Using the process of pre-plating nickel layer, plating phosphorus-containing base nickel layer and plating matte nickel layer, a matte mist coating is prepared through components such as nickel sulfamate and nickel chloride, avoiding the use of matte nickel additives, and regulating the pH value and Wetting agent concentration to reduce coating tension and porosity and improve corrosion resistance and ductility.
It achieves the electroplating of completely matte, good ductility, low stress, and low porosity matte nickel coating without the need for matte nickel additives, which reduces production costs, improves plating efficiency and process controllability, and avoids high frequency Maintenance operations.
Smart Images

Figure CN118773683A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nickel electroplating, and in particular to a process for electroplating matte nickel. Background Art
[0002] The existing matte nickel solution is mainly a nickel sulfate system, and the softness and ductility of the nickel sulfate system coating are poorer than those of the aminosulfonic acid nickel system, and the operable current density range is narrower. At the same time, this electroplating system usually prepares the matte nickel coating by adding matte nickel additives such as polyethylene glycol and quaternary ammonium salt compounds to the electroplating solution. However, during the electroplating process, the matte nickel additive is continuously consumed and decomposed, and the consumption concentration of the matte nickel additive is difficult to control. The concentration of the matte nickel additive directly affects the appearance of the coating, and there is a risk of unstable appearance.
[0003] In addition, the consumption and decomposition of matte nickel additives produce ineffective substances, which remain in the electroplating solution and affect the electroplating bonding and various quality problems. Hydrogen peroxide and activated carbon must be regularly used for maintenance. The treatment process is cumbersome and time-consuming, affecting the electroplating efficiency. Therefore, it is of great significance to develop a process that can achieve matte nickel plating without matte nickel additives. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a matte nickel electroplating process, in which a completely matte, ductile, low-stress, and low-porosity matte nickel plating layer is electroplated through a pre-nickel layer, a phosphorus-containing base nickel layer, and a matte nickel layer. No matte nickel additive is required to be added to the electroplating solution, and the appearance and quality of the matte nickel layer are not affected by the concentration of the matte nickel additive. No high-frequency maintenance operation is required, the process controllability is good, and the electroplating efficiency is high.
[0005] In order to solve the above technical problems, the present invention provides a frosted nickel electroplating process, comprising the following steps:
[0006] S1, pre-nickel plating: placing the workpiece in a first electroplating solution as a cathode pre-nickel plating layer, wherein the first electroplating solution comprises nickel sulfamate, sulfamic acid and water;
[0007] S2, plating a phosphorus-containing primer nickel layer: placing the workpiece with the pre-nickel layer in a second electroplating solution, as a cathode, electroplating the phosphorus-containing primer nickel layer, wherein the components of the second electroplating solution are: nickel sulfamate, nickel chloride, boric acid, aminosulfonic acid, a phosphorus-containing additive, a wetting agent and water;
[0008] S3, plating a matte nickel layer: placing the workpiece electroplated with a phosphorus-containing primer nickel layer in a third electroplating solution as a cathode for electroplating a matte nickel layer, wherein the components of the third electroplating solution are: nickel sulfamate, nickel chloride, boric acid, aminosulfonic acid, a wetting agent and water.
[0009] The present invention uses an aqueous solution of nickel sulfamate to pre-plated nickel layer. Compared with the pre-plated nickel layer using hydrochloric acid and nickel chloride, the coating prepared by the first electroplating solution of the present invention is matte and misty, and the coating stress is small, which lays a good foundation for the subsequent electroplating of matte nickel. The present invention electroplates a phosphorus-containing primer nickel layer between the pre-plated nickel layer and the matte nickel layer, and regulates the concentration of nickel sulfamate and phosphorus-containing additives in the second electroplating solution, while leveling the coating and improving the corrosion resistance of the coating without significantly improving the gloss of the coating. When electroplating the matte nickel layer, no polyethylene glycol, quaternary ammonium salt compounds and other matte nickel additives are added to the electroplating solution. In addition to nickel sulfamate and nickel chloride providing nickel elements, and sulfamate and boric acid adjusting pH, only a wetting agent is added to reduce the tension and porosity of the coating, without the need for high-frequency maintenance, reducing production costs, and improving electroplating efficiency. At the same time, a relatively low pH value is controlled to make the coating crystal particles more delicate without affecting the normal electroplating efficiency.
[0010] Further, the concentration of nickel sulfamate in the first electroplating solution is 80-100 g / L, and the pH is adjusted to 0.9-1.5 by sulfamate;
[0011] The concentration of nickel sulfamate in the second electroplating solution is 55-65 g / L, the concentration of nickel chloride is 9-17 g / L, the concentration of the phosphorus-containing additive is 3-7 g / L, the wetting agent is 1.5-2.5 g / L, the pH is adjusted to 1.5-2.5 by sulfamate, and the acid-base balance is maintained by boric acid;
[0012] The concentration of nickel sulfamate in the third electroplating solution is 80-100 g / L, the concentration of nickel chloride is 9-17 g / L, the wetting agent is 1.5-2.5 g / L, the pH is adjusted to 2.8-3.2 by sulfamate, and the acid-base balance is maintained by boric acid.
[0013] Furthermore, the phosphorus-containing additive is an aqueous solution of sodium hypophosphite and / or phosphorous acid.
[0014] Furthermore, the wetting agent is sodium lauryl sulfate.
[0015] Furthermore, the thicknesses of the pre-plated nickel layer and the phosphorus-containing primer nickel layer are independently 0.1-0.3 μm, and the thickness of the matte nickel layer is 2-5 μm.
[0016] Furthermore, the cathode current density in S1 is 6-8 ASD, the cathode current density in S2 is 2.5-5 ASD, and the cathode current density in S3 is 10-15 ASD.
[0017] Furthermore, the temperatures of the first electroplating solution, the second electroplating solution and the third electroplating solution are independently 55-65° C.
[0018] Furthermore, the pre-nickel plating step also includes a polishing step: the workpiece is used as an anode, the voltage of the power supply is 1.5-2.5V, and the hydrochloric acid aqueous solution is used for polishing, wherein the mass concentration of the hydrochloric acid in the solution is 13%-23%.
[0019] Furthermore, the polishing step also includes a degreasing step before the polishing step: immersing the workpiece as a cathode in a degreasing agent aqueous solution with a concentration of 70-110 g / L, and performing degreasing treatment under the conditions of cathode current density of 8-15 ASD and temperature of 60-80°C.
[0020] Furthermore, the degreasing agent is one or a combination of sodium hydroxide, sodium phosphate, sodium carbonate, and polyoxyethylene fatty alcohol ether.
[0021] Beneficial effects of the present invention:
[0022] The present invention does not need to add a matte nickel additive to the electroplating solution, and electroplates a matte nickel coating with a completely matte finish, good ductility, low stress, and low porosity. The appearance and quality of the matte nickel layer are not affected by the concentration of the matte nickel additive, and does not require high-frequency maintenance operations. The process controllability is good and the electroplating efficiency is high.
[0023] The present invention adopts an aqueous solution of nickel sulfamate to pre-plated nickel layer. Compared with the pre-plated nickel layer using hydrochloric acid and nickel chloride, the pre-plated nickel layer of the present invention is matte and has low plating stress, thus laying a good foundation for subsequent electroplating of matte nickel.
[0024] The present invention electroplates a phosphorus-containing primer nickel layer between the pre-plated nickel layer and the matte nickel layer, which can level the plated layer and improve the corrosion resistance of the plated layer without significantly improving the glossiness of the plated layer.
[0025] When electroplating a matte nickel layer, the present invention does not add a matte nickel additive such as polyethylene glycol or a quaternary ammonium salt compound to the electroplating solution. In addition to nickel sulfamate and nickel chloride providing nickel elements, and sulfamate and boric acid adjusting pH, only a wetting agent is added to reduce the tension and porosity of the coating, and high-frequency maintenance is not required, the production cost is reduced, and the electroplating efficiency is improved. Meanwhile, a suitable pH value is controlled, and the crystal particles of the coating are made finer without affecting the normal electroplating efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a comparison diagram of the Hastelloy sheet of the electroplated matte nickel workpiece in Example 1 of the present invention;
[0027] Figure 2 This is a comparison diagram of the Hastelloy sheet of the electroplated matte nickel workpiece of Comparative Example 1 of the present invention;
[0028] Figure 3 This is a 20x microscope photo of the matte nickel electroplated workpiece in Example 1 of the present invention;
[0029] Figure 4This is a 20x microscope photo of a matte nickel electroplated workpiece in Comparative Example 1 of the present invention;
[0030] Figure 5 In the figure, a and b are photographs of the 90° bending of the electroplated matte nickel workpieces of Example 1 and Comparative Example 1; c and d are photographs of the electroplated matte nickel workpieces of Example 1 and Comparative Example 1 after tinning; e and f are photographs of the electroplated matte nickel workpieces of Example 1 and Comparative Example 1 after 8 hours of neutral salt spray test. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0032] Example 1
[0033] This embodiment relates to a frosted nickel electroplating process, comprising the following steps:
[0034] S1. Degreasing step: immerse the workpiece as a cathode in a degreasing agent aqueous solution with a concentration of 90 g / L, and degrease for 40 seconds at a cathode current density of 8-15 ASD and a temperature of 60-80°C, wherein the degreasing agent is a mixture of sodium hydroxide, sodium phosphate, sodium carbonate, and polyoxyethylene fatty alcohol ether in a mass ratio of 60:9.5:30:0.5.
[0035] S2, polishing step: the degreased workpiece is used as an anode, the voltage of electricity is 1.5-2.5V, and a hydrochloric acid aqueous solution is used for polishing, wherein the mass concentration of the hydrochloric acid in the solution is 18%.
[0036] S3, pre-nickel plating layer: place the workpiece in the first electroplating solution as a cathode 55-65°C pre-nickel plating layer, the first electroplating solution comprises nickel sulfamate, sulfamic acid and water, wherein the concentration of nickel sulfamate in the first electroplating solution is 90g / L, the pH is adjusted to 1.2 by sulfamic acid, the cathode current density is 6-8ASD, the electroplating time is 8s, and the thickness of the pre-nickel plating layer is 0.1-0.3μm.
[0037] S4, plating a phosphorus-containing primer nickel layer: placing the workpiece with the pre-nickel layer in a second electroplating solution, as a cathode, electroplating the phosphorus-containing primer nickel layer at 55-65°C, the components of the second electroplating solution are: nickel sulfamate, nickel chloride, boric acid, sulfamate, a phosphorus-containing additive (aqueous solution of phosphorous acid with a mass concentration of 15%), sodium dodecyl sulfate and water, wherein the concentration of nickel sulfamate in the second electroplating solution is 60g / L, the concentration of nickel chloride is 13g / L, the concentration of the phosphorus-containing additive is 5g / L, the concentration of sodium dodecyl sulfate is 2g / L, the pH is 2 through sulfamate, and the acid-base balance is maintained by boric acid, the cathode current density is 2.5-5ASD, the electroplating time is 8s, and the thickness of the pre-nickel plating layer is 0.1-0.3μm.
[0038] S5. Matte nickel plating: Place the workpiece plated with a phosphorus-containing base nickel layer in a third electroplating solution, and use it as a cathode to electroplate a matte nickel layer at 55-65°C. The components of the third electroplating solution are: nickel sulfamate, nickel chloride, boric acid, sulfamate, sodium dodecyl sulfate and water. The concentration of nickel sulfamate in the third electroplating solution is 90g / L, the concentration of nickel chloride is 13g / L, and the concentration of sodium dodecyl sulfate is 2g / L. The pH value is 3 through sulfamate, and the acid-base balance is maintained by boric acid. The cathode current density is 10-15ASD, the electroplating time is 70s, and the thickness of the pre-nickel plating layer is 2-3μm.
[0039] Comparative Example 1
[0040] The steps S1 and S2 of this comparative example and embodiment 1 are the same as those of embodiment 1, except that S3 is a pre-nickel plating layer, S4 is a phosphorus-containing primer nickel plating layer, and S5 is a matte nickel plating layer, specifically:
[0041] S3. Pre-nickel plating: placing the workpiece in a first electroplating solution as a cathode for pre-nickel plating at room temperature, wherein the first electroplating solution comprises hydrochloric acid, nickel chloride and water, wherein the mass concentration of hydrochloric acid in the first electroplating solution is 9%, the concentration of nickel chloride is 180 g / L, the cathode current density is 6-8 ASD, the electroplating time is 8 s, and the thickness of the pre-nickel plating layer is 0.1-0.3 μm.
[0042] S4, plating a phosphorus-containing primer nickel layer: placing the workpiece with the pre-nickel layer in a second electroplating solution, as a cathode, electroplating the phosphorus-containing primer nickel layer at 55-65°C, the components of the second electroplating solution are: nickel sulfamate, nickel chloride, boric acid, sulfamate, a phosphorus-containing additive (aqueous solution of phosphorous acid with a mass concentration of 15%), sodium dodecyl sulfate and water, wherein the concentration of nickel sulfamate in the second electroplating solution is 90g / L, the concentration of nickel chloride is 13g / L, the concentration of the phosphorus-containing additive is 20g / L, and the concentration of sodium dodecyl sulfate is 2g / L. The pH value is 2 through sulfamate, and the acid-base balance is maintained by boric acid. The cathode current density is 5-10ASD, the electroplating time is 8s, and the thickness of the pre-nickel plating layer is 0.1-0.3μm.
[0043] S5. Matte nickel plating: Place the workpiece to be plated with a phosphorus-containing base nickel layer in a third electroplating solution, and use it as a cathode to electroplate a matte nickel layer at 55-65°C. The components of the third electroplating solution are: nickel sulfamate, nickel chloride, a matte nickel additive (a quaternary ammonium salt compound aqueous solution with a mass concentration of 20%), boric acid, sulfamate, sodium dodecyl sulfate and water. The concentration of nickel sulfamate in the third electroplating solution is 90g / L, the concentration of nickel chloride is 13g / L, the concentration of the matte nickel additive is 1g / L, and the concentration of sodium dodecyl sulfate is 2g / L. The pH value is 3 through sulfamate, and the acid-base balance is maintained through boric acid. The cathode current density is 10-15ASD, the electroplating time is 70s, and the thickness of the pre-nickel plating layer is 2-3μm.
[0044] Test Case
[0045] The matte nickel electroplating workpieces prepared in the embodiment and the comparative example were compared with the Hastelloy sheet. The results showed that the matte nickel electroplating workpiece of the comparative example 1 was in the fog zone at a current density of more than 4. Figure 2 , and in this embodiment, the current density is above 3, which is the fog area, refer to Figure 1 Meanwhile, in comparative example 1, when the matte nickel layer is plated, a matte nickel additive is added, and the concentration of the additive needs to be regularly detected and maintained, resulting in low working efficiency.
[0046] The electroplated matte nickel workpieces prepared in the examples and comparative examples were placed under a 20x microscope for observation. Figure 3 and 4 As shown, by comparing the two photos, it is found that the coatings of Example 1 and Comparative Example 1 are both foggy in appearance, but the coating prepared in Example 1 is fine and uniform.
[0047] The electroplated matte nickel workpieces prepared in the examples and comparative examples were subjected to a 90-degree bending test, a tinning test, and a neutral salt spray test for 8 hours. Figure 5 As shown in af, after the workpieces of Example 1 and Comparative Example 1 electroplated with matte nickel were bent at 90 degrees, the coating was firm and there was no peeling under a 10x microscope, and the test was OK; the workpieces of Example 1 and Comparative Example 1 electroplated with matte nickel were subjected to a tin wetting test, and the tin wetting area was observed under a microscope to be more than 95%, and the test was OK; the workpieces of Example 1 and Comparative Example 1 electroplated with matte nickel were subjected to neutral salt spray conditions for 8 hours, and there was no corrosion observed under a 10x microscope.
[0048] In summary, the present invention does not need to add matte nickel additives to the electroplating solution, and can electroplate a completely matte, ductile, low-stress, and low-porosity matte nickel coating. The appearance and quality of the matte nickel layer are not affected by the concentration of the matte nickel additive, and does not require high-frequency maintenance operations. The process has good controllability, can achieve continuous production, and has high electroplating efficiency.
[0049] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A frosted nickel electroplating process, characterized in that: The steps include: S1, pre-nickel plating: placing the workpiece in a first electroplating solution as a cathode pre-nickel plating layer, wherein the first electroplating solution comprises nickel sulfamate, sulfamic acid and water; S2, plating a phosphorus-containing primer nickel layer: placing the workpiece with the pre-nickel layer in a second electroplating solution, as a cathode, electroplating the phosphorus-containing primer nickel layer, wherein the components of the second electroplating solution are: nickel sulfamate, nickel chloride, boric acid, aminosulfonic acid, a phosphorus-containing additive, a wetting agent and water; S3, plating a matte nickel layer: placing the workpiece electroplated with a phosphorus-containing primer nickel layer in a third electroplating solution as a cathode for electroplating a matte nickel layer, wherein the components of the third electroplating solution are: nickel sulfamate, nickel chloride, boric acid, aminosulfonic acid, a wetting agent and water.
2. The electroplating process for matte nickel according to claim 1, characterized in that: The concentration of nickel sulfamate in the first electroplating solution is 80-100 g / L, and the pH is 0.9-1.5; The concentration of nickel sulfamate in the second electroplating solution is 55-65 g / L, the concentration of nickel chloride is 9-17 g / L, the concentration of the phosphorus-containing additive is 3-7 g / L, the wetting agent is 1.5-2.5 g / L, and the pH is 1.5-2.5; The concentration of nickel sulfamate in the third electroplating solution is 80-100 g / L, the concentration of nickel chloride is 9-17 g / L, the wetting agent is 1.5-2.5 g / L, and the pH is 2.8-3.
2.
3. The electroplating process for matte nickel according to claim 1, characterized in that: The phosphorus-containing additive is an aqueous solution of sodium hypophosphite and / or phosphorous acid.
4. The electroplating process for matte nickel according to claim 1, characterized in that: The wetting agent is sodium lauryl sulfate.
5. The electroplating process for matte nickel according to claim 1, characterized in that: The thickness of the pre-plated nickel layer and the phosphorus-containing primer nickel layer are independently 0.1-0.3 μm, and the thickness of the matte nickel layer is 2-5 μm.
6. The electroplating process for matte nickel according to claim 1, characterized in that: The cathode current density in S1 is 6-8 ASD, the cathode current density in S2 is 2.5-5 ASD, and the cathode current density in S3 is 10-15 ASD.
7. The electroplating process for matte nickel according to claim 1, characterized in that: The temperatures of the first electroplating solution, the second electroplating solution and the third electroplating solution are independently 55-65° C.
8. The electroplating process for matte nickel according to claim 1, characterized in that: The process also includes a polishing step before the nickel pre-plating: using the workpiece as an anode, applying a voltage of 1.5-2.5V, and polishing with a hydrochloric acid aqueous solution, wherein the mass concentration of the hydrochloric acid in the solution is 13%-23%.
9. The electroplating process for matte nickel according to claim 8, characterized in that: The polishing step also includes a degreasing step: immersing the workpiece as a cathode in a degreasing agent aqueous solution with a concentration of 70-110 g / L, and performing degreasing treatment under the conditions of a cathode current density of 8-15 ASD and a temperature of 60-80°C.
10. The electroplating process for matte nickel according to claim 9, characterized in that: The degreasing agent is one or a combination of sodium hydroxide, sodium phosphate, sodium carbonate and polyoxyethylene fatty alcohol ether.
Citation Information
Cited By
Nickel plating process and pre-electroplating lead frame
CN120649103A