Laminated substrate
By selectively adding carbon doping raw material gas in the peripheral area of the GaN stacked substrate, the problem of carrier concentration non-uniformity caused by the non-uniform silicon concentration distribution is solved, and the uniformity of the GaN layer and the performance of the semiconductor device are improved. .
Patent Information
- Application Number
- CN202410391009.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-15
AI Technical Summary
In large-diameter gallium nitride (GaN) laminated substrates, there is in-plane inhomogeneity in the silicon (Si) concentration distribution, resulting in in-plane inhomogeneity in n-type carrier concentration and affecting the performance of semiconductor devices.
By introducing carbon (C) doped raw material gas on the upper surface of the GaN layer, the excess n-type carrier concentration is selectively compensated in the peripheral area, and the distribution of carbon is used to uniformize the silicon concentration distribution, thereby reducing the Si concentration between the center and the periphery. concentration difference.
The in-plane non-uniformity of n-type carrier concentration caused by Si concentration distribution is effectively suppressed, and the uniformity of the GaN layer and the performance of the semiconductor device are improved.
Smart Images

Figure CN118773731A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminate substrate. Background Art
[0002] A stacked substrate having a gallium nitride (GaN) layer epitaxially grown on various base substrates is used as a material for manufacturing semiconductor devices (for example, see Patent Document 1). In order to improve the production efficiency of semiconductor devices, the stacked substrate is being enlarged. Silicon (Si) is used as an n-type impurity added to the GaN layer.
[0003] As described in detail later, the inventors conducted research on a stacked substrate with a large diameter, a low added Si concentration and a thick GaN layer, and found that in-plane unevenness of the Si concentration distribution in the GaN layer (specifically, unevenness such that the Si concentration becomes higher on the outer peripheral side of the GaN layer) is easily produced.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-199601 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] An object of the present invention is to provide a multilayer substrate in which in-plane nonuniformity of n-type carrier concentration caused by in-plane nonuniformity of Si concentration distribution in a GaN layer is suppressed.
[0009] Solutions for solving problems
[0010] According to one embodiment of the present invention, there is provided a laminate substrate comprising:
[0011] a base substrate; and
[0012] a gallium nitride layer epitaxially grown on the base substrate and composed of gallium nitride doped with silicon,
[0013] The gallium nitride layer has an upper surface with a radius of more than 50 mm,
[0014] The thickness of the gallium nitride layer is greater than 4 μm,
[0015] The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central silicon concentration at the center of the upper surface.
[0016] The central silicon concentration is 4×10 15 cm -3More than and less than 2×10 16 cm -3 ,
[0017] The carbon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral carbon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central carbon concentration at a center of the upper surface.
[0018] Effects of the Invention
[0019] The present invention provides a multilayer substrate in which in-plane nonuniformity of n-type carrier concentration caused by in-plane nonuniformity of Si concentration distribution in a GaN layer is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic cross-sectional view of a laminated substrate according to an exemplary embodiment.
[0021] Figure 2 This is a top view of a GaN layer for explaining a method for measuring the Si concentration and the C concentration in the GaN layer.
[0022] Figure 3 It is a schematic side view showing a GaN layer manufacturing apparatus according to an embodiment.
[0023] Figure 4 This is a graph showing an example of the C concentration distribution on the upper surface of the GaN layer according to the embodiment.
[0024] Figure 5 It is a timing chart schematically showing the supply mode of the C-doped raw material gas at a representative position of the periphery.
[0025] Figure 6 This is a schematic cross-sectional view of a GaN layer according to an exemplary embodiment.
[0026] Figure 7 It is a schematic side view showing a manufacturing apparatus of a GaN layer of a comparative method.
[0027] Figure 8 This is a graph showing an example of Si concentration distribution on the upper surface of the GaN layer according to the embodiment or the comparative embodiment.
[0028] Description of Reference Numerals
[0029] 10…Base structure, 20…GaN layer, 21…Region without C addition, 22…Region with C addition, 23…Region with low Si concentration, 24…Region with high Si concentration, 25…Upper surface (of GaN layer), 30…Upper layer, 40…Wafer, 100…Laminated substrate, 200…Manufacturing device, 210…Susceptor, 211…Inner periphery of susceptor, 212…Outer periphery of susceptor, 213…Upper surface of susceptor edge, 220…(Main) raw material gas, 230…Si-containing deposit, 240…Raw material gas for compensation DETAILED DESCRIPTION
[0030] A laminated substrate 100 according to an embodiment of the present invention will be described. Figure 1 1 is a schematic cross-sectional view illustrating a laminate substrate 100 . The laminate substrate 100 includes at least a base structure 10 and a gallium nitride (GaN) layer 20 formed on the base structure 10 .
[0031] The base structure 10 has at least a base substrate as a crystal substrate for epitaxially growing the GaN layer 20. The base structure 10 may also have a buffer layer between the base substrate and the GaN layer 20 as required. The structure of the buffer layer can be appropriately selected as required.
[0032] As the base substrate, a GaN substrate, a sapphire substrate, a silicon (Si) substrate, a silicon carbide (SiC) substrate, etc. can be appropriately used. For example, when the base substrate is a GaN substrate, the base structure 10 can be a GaN substrate. In addition, for example, when the base substrate is a Si substrate, the base structure 10 can have a Si substrate and an aluminum nitride (AlN) layer provided as a nucleation layer, etc.
[0033] The laminated substrate 100 may include an upper layer 30 formed on the GaN layer 20 as required. The structure of the upper layer 30 may be appropriately selected according to the operation of the semiconductor device to be manufactured using the laminated substrate 100. The upper layer 30 may be, for example, a group III nitride layer epitaxially grown on the GaN layer 20.
[0034] The GaN layer 20 of the embodiment has the following features. The GaN layer 20 has an upper surface 25 with a radius of 50 mm or more (a diameter of 100 mm or more). That is, the laminated substrate 100 has a circular shape with a diameter of 100 mm or more. It should be noted that the laminated substrate 100 may have a positioning plane or a notch as needed.
[0035] GaN layer 20 contains silicon (Si) as an n-type impurity. The Si concentration of upper surface 25 of GaN layer 20 has a distribution in which a peripheral Si concentration CSi1 at the periphery of upper surface 25 is higher than a central Si concentration CSi0 at the center of upper surface 25 .
[0036] The central Si concentration CSi0 is 10 15 cm -3 The concentration change of the order of magnitude will have an impact on the low concentration, specifically, 4×10 15 cm -3 More than and less than 2×10 16 cm -3 The Si concentration CSi0 in the center is less than 1×10 16 cm -3 (i.e. 10 15 cm -3 In the case of the method of the order of magnitude of , such influence is more significant. The thickness of the GaN layer 20 is 4 μm or more. In addition, the thickness of the GaN layer 20 is, for example, 40 μm or less.
[0037] The GaN layer 20 is a layer that functions as at least a part of the operating layer in the semiconductor element formed by the stacked substrate 100. Therefore, the GaN layer 20 preferably has both withstand voltage characteristics and resistance characteristics in a balanced manner. From the perspective of improving the withstand voltage, the central Si concentration CSi0 of the GaN layer 20 is preferably less than 2×10 16 cm -3 In addition, from the viewpoint of increasing the withstand voltage, the thickness of the GaN layer 20 is preferably 4 μm or more. From the viewpoint of reducing the resistance, the central Si concentration CSi0 of the GaN layer 20 is preferably 4×10 15 cm -3 Furthermore, from the viewpoint of reducing the resistance, the thickness of the GaN layer 20 is preferably 40 μm or less.
[0038] As described later, the peripheral Si mixed concentration (i.e., CSi1-CSi0), which is the excess amount of the peripheral Si concentration CSi1 over the central Si concentration CSi0, is the concentration of Si mixed into the periphery of the GaN layer 20 due to the Si-containing deposit 230. The central Si concentration CSi0 is substantially equal to the target added concentration, which is the concentration of Si added intentionally.
[0039] Due to the mixing of Si, the n-type carrier concentration at the periphery exceeds that at the center. In the GaN layer 20, carbon (C) is contained as an impurity to compensate for the excess n-type carrier concentration at the periphery. The C concentration of the upper surface 25 of the GaN layer 20 has the following distribution: the peripheral C concentration CC1 at the periphery of the upper surface 25 is high relative to the central C concentration CC0 at the center of the upper surface 25. The peripheral C added concentration (i.e., CC1-CC0), which is the excess of the peripheral C concentration CC1 over the central C concentration CC0, is the concentration of C added in a manner to compensate for the excess n-type carrier concentration at the periphery.
[0040] In the following description, the radius of the GaN layer 20 is 50 mm, the thickness of the GaN layer 20 is 4 μm, and the target concentration of Si added in the GaN layer 20 is 9×10 15 cm -3 way.
[0041] The following describes a method for measuring the Si concentration and the C concentration in the GaN layer 20. In order to avoid cumbersome descriptions, the common contents of the Si concentration and the C concentration are sometimes expressed simply as concentration. Figure 2 1 is a plan view of the GaN layer 20 for explaining a method of measuring the concentration in the GaN layer 20. An XY orthogonal coordinate system is set on the upper surface 25 of the GaN layer 20, with the center of the upper surface 25 as the origin.
[0042] First, the measurement positions within the surface are described. As measurement points for the concentration on the upper surface 25, at least a central measurement point and four peripheral measurement points, a total of five measurement points, are set. The central measurement point is set at the center of the upper surface 25. The four peripheral measurement points are set at radial positions 10 mm from the edge of the upper surface 25 for the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction (i.e., every 90° along the circumferential direction). Here, as a representative position of the periphery when specifying the concentration at the periphery of the upper surface 25, a radial position 10 mm from the edge of the upper surface 25 is set.
[0043] The Si concentration at the central measurement point is the central Si concentration CSi0. The Si concentration obtained by averaging the Si concentration CSiX+ of the peripheral measurement point in the positive X direction, the Si concentration CSiX- of the peripheral measurement point in the negative X direction, the Si concentration CSiY+ of the peripheral measurement point in the positive Y direction, and the Si concentration CSiY- of the peripheral measurement point in the negative Y direction is the peripheral Si concentration CSi1. That is, the peripheral Si concentration CSi1 represents the Si concentration averaged in the peripheral direction. The excess of the peripheral Si concentration CSi1 over the central Si concentration CSi0, that is, CSi1-CSi0, is the peripheral Si mixing concentration.
[0044] The C concentration at the central measurement point is the central C concentration CC0. The C concentration CCX+ of the peripheral measurement point in the positive X direction, the C concentration CCX- of the peripheral measurement point in the negative X direction, the C concentration CCY+ of the peripheral measurement point in the positive Y direction, and the C concentration CCY- of the peripheral measurement point in the negative Y direction are averaged to form the peripheral C concentration CC1. That is, the peripheral C concentration CC1 represents the C concentration averaged in the peripheral direction. The excess of the peripheral C concentration CC1 over the central C concentration CC0, that is, CC1-CC0, is the peripheral C added concentration.
[0045] In this example, the radius of the upper surface 25 is 50 mm. Four outer periphery measurement points are set at radial positions 40 mm from the center in the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction.
[0046] In addition to the central measurement point and the four peripheral measurement points, an intermediate measurement point can also be set at a radial position between the central measurement point and the peripheral measurement point. In this example, the intermediate measurement point is set at a radial position of 10 mm, 20 mm, and 30 mm from the center for the positive X direction, negative X direction, positive Y direction, and negative Y direction, respectively. Figure 2 In order to facilitate illustration, large black dots are used to represent the central measurement points and the peripheral measurement points, and small black dots are used to represent the intermediate measurement points.
[0047] It should be noted that, in the case where the radius of the upper surface 25 of the GaN layer 20 exceeds 50 mm, the four peripheral measurement points are also set at radial positions 10 mm from the edge of the upper surface 25. In addition, in the case where the radius of the upper surface 25 of the GaN layer 20 exceeds 50 mm, the intermediate measurement points may also be set at radial positions every 10 mm from the center for the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction.
[0048] The concentration obtained by averaging the concentrations at four measurement points in the positive X direction, the negative X direction, the positive Y direction, and the negative Y direction set at equal radial positions from the center of the upper surface 25, that is, the concentration averaged circumferentially at each radial position, is referred to as the average Si concentration and the average C concentration for Si and C, respectively. The peripheral Si concentration CSi1 and the peripheral C concentration CC1 are the average Si concentration and the average C concentration at the periphery, respectively.
[0049] As described later, the growth of the GaN layer 20 is carried out in a manner that is uniform in the circumferential direction. However, in reality, even between the four measurement points set at equal radial positions, there will be concentration deviations. In order to reduce the impact of this deviation, for Si and C, the Si concentration obtained by circumferential averaging, that is, the average Si concentration, and the C concentration obtained by circumferential averaging, that is, the average C concentration, are used to evaluate the radial distribution of the concentration in the GaN layer 20. The concentration of mixed Si is the excess of the average Si concentration at each radial position over the central Si concentration CSi0. The concentration of added C is the excess of the average C concentration at each radial position over the central C concentration CC0.
[0050] It should be noted that when it is stipulated that "the peripheral Si concentration CSi1 is higher than the central Si concentration CSi0", not only the condition that the peripheral Si concentration CSi1, that is, the average value of the Si concentration at the four peripheral measurement points is higher than the central Si concentration CSi0, but also the condition that the Si concentration of at least three (preferably four) of the four peripheral measurement points is higher than the central Si concentration CSi0.
[0051] In addition, when it is stipulated that "peripheral C concentration CC1 is higher than central C concentration CC0", not only the condition that peripheral C concentration CC1, that is, the average value of the C concentration at four peripheral measurement points is higher than the central C concentration CC0, but also the condition that at least three (preferably four) of the four peripheral measurement points have C concentrations higher than the central C concentration CC0.
[0052] Next, the measurement position in the height direction is described. As the concentration in the GaN layer 20 (Si concentration and C concentration, respectively), the concentration of the upper surface 25 is measured by secondary ion mass spectrometry (SIMS). Among them, the "concentration of the upper surface 25" is not exactly the concentration at the height of the upper surface 25, but refers to the concentration near the upper surface 25 as described below. In the mode where the upper layer 30 is not stacked, the upper surface 25 is the uppermost surface of the stacked substrate 100, and in the mode where the upper layer 30 is stacked, the upper surface 25 is the interface between the upper layer 30 and the GaN layer 20.
[0053] In general, the reliability of SIMS measurement at the surface position is not high. Therefore, it is preferred to perform SIMS measurement at a height slightly from the upper surface 25 to the side of the base structure 10, that is, slightly inside the GaN layer 20. In addition, it is preferred to use a measurement value obtained by averaging a certain degree of height range (depth range, thickness range). Here, for each measurement point in the surface, the value obtained by averaging the SIMS measurement values within a depth range of more than 100nm and less than 200nm from the upper surface 25 is defined as the concentration of the upper surface 25. For example, in a method in which the thickness of the GaN layer 20 is 4μm, the average value of the concentration based on SIMS measurement in a range of more than 3.8μm and less than 3.9μm from the lower surface of the GaN layer 20 is defined as the concentration of the upper surface 25.
[0054] It should be noted that the concentration at the height between the upper surface 25 of the GaN layer 20 and the lower surface of the GaN layer 20 (the concentration at a predetermined depth position from the upper surface 25 of the GaN layer 20) is specified based on the concentration of the upper surface 25. Specifically, the value obtained by averaging the SIMS measurement values in a depth range of 100 nm to 200 nm from the predetermined depth position is specified as the concentration at the predetermined depth position.
[0055] Before further describing the embodiment, a comparative method will be described. Figure 7 1 is a schematic side view of a manufacturing apparatus 200 for manufacturing a GaN layer 20 in a comparative manner. The manufacturing apparatus 200 is a metal organic vapor phase epitaxy (MOVPE) apparatus having a susceptor 210 for mounting a wafer 40. The wafer 40 is an object to be processed (an intermediate of the laminated substrate 100) in the stage of the growth processing of the GaN layer 20 by the manufacturing apparatus 200, and specifically, is the base structure 10 at the start of the growth of the GaN layer 20, and is a laminate of the base structure 10 and the GaN layer 20 after the growth of the GaN layer 20 starts.
[0056] The manufacturing device 200 is a cross-flow MOVPE device that supplies a raw material gas 220 in a direction parallel to the upper surface of the wafer 40. The raw material gas 220 includes a GaN raw material gas for growing GaN constituting the GaN layer 20, and a Si doping raw material gas for supplying Si added to the GaN layer 20. The GaN raw material gas includes a gallium (Ga) raw material gas and a nitrogen (N) raw material gas. As the Ga raw material gas, for example, trimethyl gallium (TMG) gas is used, and as the N raw material gas, for example, ammonia (NH3) gas is used. As the Si doping raw material gas, for example, silane (SiH4) gas is used.
[0057] The growth temperature can be selected in the range of 900°C to 1400°C, for example, and the flow rate ratio of the V group source gas to the III group source gas, i.e., the V / III ratio, can be selected in the range of 10 to 5000, for example. The Si doping source gas is added to the GaN layer 20 at a target concentration of 4×10 15 cm -3 More than and less than 2×10 16 cm -3 A specified value within the range of 9×10 15 cm -3 supplied in the form of .
[0058] The susceptor 210 holds the wafer 40 so as to rotate the wafer 40 about the center of the wafer 40 . By growing the GaN layer 20 while performing such rotation, the growth conditions of the GaN layer 20 are made uniform in the circumferential direction of the wafer 40 .
[0059] The susceptor inner peripheral edge 211 is a position of the edge of the susceptor 210 where the wafer 40 is placed in a plan view. The susceptor edge upper surface 213 is an upper surface of the susceptor 210 between the susceptor inner peripheral edge 211 and the susceptor outer peripheral edge 212 .
[0060] As the GaN layer 20 grows, the Si-containing deposit 230 adheres to the upper surface 213 of the susceptor edge, so that Si is mixed into the GaN layer 20 from the Si-containing deposit 230. The inclusion of Si in the GaN layer 20 due to the Si-containing deposit 230 is referred to as "mixing", which is distinguished from "addition" in which the GaN layer 20 is intentionally made to contain Si by Si-doping raw material gas. The Si concentration of the upper surface 25 of the GaN layer 20 becomes the sum of the concentration of Si added by the Si-doping raw material gas and the concentration of Si mixed by the Si-containing deposit 230.
[0061] The concentration of Si added by the Si doping source gas is schematically constant over the entire region of the upper surface 25 of the GaN layer 20. The concentration of Si mixed in by the Si-containing deposit 230 increases as the position closer to the susceptor inner periphery 211, that is, closer to the outer periphery of the edge of the wafer 40.
[0062] Figure 8 1 is a graph showing an example of Si concentration distribution on the upper surface 25 of the GaN layer 20 of the comparative method. The horizontal axis represents the measurement position in the plane in mm units, and the vertical axis represents the measurement position in 10 15 cm -3 The unit represents Si concentration. The Si concentration at each measurement point in the X direction is represented by a black circle, and the Si concentration at each measurement point in the Y direction is represented by a hollow rectangle. The average Si concentration is represented by a cross.
[0063] It should be noted that, here, a method in which C is not added in the embodiment described later is described as a comparative method. Therefore, except that C is not added, the comparative method is the same as the embodiment. Figure 8 The Si concentration distribution shown is the same in the comparative embodiment and the embodiment.
[0064] The central Si concentration CSi0 is 9×10 15 cm -3 Roughly equal, 9.01×10 15 cm -3 Furthermore, the Si concentration at a distance of about 10 mm from the center is substantially constant. Therefore, it can be said that the mixed Si does not reach the center of the wafer 40 .
[0065] At radial positions about 20 mm from the center, the excess of the central Si concentration CSi0, i.e., the concentration of the mixed Si, becomes significantly higher. In addition, the concentration of the mixed Si increases as it approaches the outer periphery. The outer Si concentration CSi1 is 10.65×10 15 cm -3 The excess of the peripheral Si concentration CSi1 over the central Si concentration CSi0, i.e., the peripheral Si mixing concentration, is 1.64×10 15cm -3 .
[0066] Si caused by the Si-containing deposit 230 is mixed into a width of about 40 mm in the radial direction from the edge of the wafer 40. In the case of a large-diameter wafer 40, such as a 50 mm radius, as in this example, Si mixing does not occur at the center. On the other hand, if a method is used in which a wafer with a smaller diameter, such as a 25 mm radius, is used, Si mixing will also occur at the center of the wafer.
[0067] In the case of a small diameter structure where Si is mixed in the center, mixed Si from both sides of the center overlaps in the center, so that the Si concentration caused by the mixed Si also becomes high in the center. As a result, the Si concentration distribution caused by the mixed Si becomes nearly uniform in the plane.
[0068] In contrast, in a large-diameter wafer 40 where Si is not mixed in the center as in this example, the Si concentration distribution caused by the mixed Si becomes a non-uniform distribution with a large difference between the center and the periphery. Thus, in a large-diameter wafer 40, specifically, a wafer with a radius of 50 mm or more, the in-plane non-uniformity of the Si concentration distribution caused by the mixed Si becomes significant.
[0069] Although the example of a 50 mm radius is described, in the case of a wafer 40 having a radius exceeding 50 mm, the concentration of mixed Si at the outer periphery (a radial position 10 mm from the edge of the wafer 40 ) is also at the same level as that of the 50 mm radius.
[0070] The peripheral Si concentration, which is the difference between the center and the periphery, is 1.64×10 15 cm -3 On the other hand, the target Si addition concentration, i.e., the center Si concentration CSi0, is 10 15 cm -3 Therefore, the influence of the peripheral Si mixed concentration on the Si concentration distribution in the plane becomes significant.
[0071] Thus, when the radius of the upper surface 25 is greater than 50 mm and the central Si concentration CSi0 is 4×10 15 cm -3 More than and less than 2×10 16 cm -3 (and thus less than 1×10 16 cm -3 ) in the GaN layer 20, the Si concentration difference between the center and the periphery caused by the mixing of Si becomes significant. That is, due to such Si concentration difference, the n-type carrier concentration difference between the center and the periphery becomes significant. As described below, in the embodiment, a technology that can suppress such n-type carrier concentration difference between the center and the periphery compared with the comparative method is proposed.
[0072] The implementation method is further described. As mentioned above, Figure 8 This is also a graph showing the Si concentration distribution on the upper surface 25 of the GaN layer 20 according to the embodiment. The Si concentration distribution will be described further.
[0073] The lower limit of the target added concentration, that is, the lower limit of the central Si concentration CSi0, is 4×10 15 cm -3 The Si concentration exceeds 10%, which is 0.4×10 15 cm -3 The region where the concentration of Si mixed is equal to or less than the concentration of Si mixed is referred to as a low concentration Si mixed region 23 . The region where the concentration of Si mixed exceeds the concentration of Si mixed is referred to as a high concentration Si mixed region 24 .
[0074] The Si high concentration region 24 is an annular region on the edge side of the upper surface 25 of the GaN layer 20. The circular region (the entire region) further inside the annular region serving as the Si high concentration region 24 is an Si low concentration region 23. The width of the annular region serving as the Si high concentration region 24 from the edge of the upper surface 25 is approximately 30 mm.
[0075] The Si-doped high concentration region 24 is a region where the excess of n-type carrier concentration caused by Si doping is large. In the embodiment, C is added to the Si-doped high concentration region 24 to compensate for at least a part of the excess of n-type carrier concentration, thereby suppressing the difference in n-type carrier concentration between the center and the periphery.
[0076] Figure 3 1 is a schematic side view of a manufacturing apparatus 200 of a GaN layer 20 according to an embodiment. The manufacturing apparatus 200 according to the embodiment is a cross-flow MOVPE apparatus similar to the comparative method, and main raw material gases 220 (GaN raw material gas and Si doping raw material gas) are supplied in a direction parallel to the upper surface of the wafer 40 .
[0077] The manufacturing apparatus 200 of the embodiment further includes a mechanism for supplying a compensating source gas 240. The compensating source gas 240 includes a C doping source gas for supplying C to be added to the GaN layer 20. As the C doping source gas, for example, methane (CH4) gas is used.
[0078] It should be noted that since the Ga raw material gas (such as TMG gas) contained in the main raw material gas 220 is an organic raw material gas, C caused by the Ga raw material gas is also contained in the GaN layer 20. The situation in which C is contained in the GaN layer 20 due to the Ga raw material gas is called "mixing", which is distinguished from "addition" in which C is intentionally contained in the GaN layer 20 by C doping the raw material gas. The C concentration on the upper surface of the GaN layer 20 becomes the sum of the concentration of C added by the C doping raw material gas and the concentration of C mixed by the Ga raw material gas.
[0079] The concentration of C mixed by the Ga source gas is schematically constant over the entire region of the upper surface 25 of the GaN layer 20. The compensation source gas 240, that is, the C doping source gas is selectively supplied to the Si high concentration region 24.
[0080] In the embodiment, in order to preferentially add C to the Si high concentration region 24, the C doping raw material gas is selectively supplied to the Si high concentration region 24, that is, in a predetermined range in the radial direction toward the outer peripheral side (in this example, specifically, a range with a width of about 30 mm from the edge of the upper surface 25). It should be noted that in the Si low concentration region 23, since the Si concentration in the outer peripheral part is slightly higher, the C doping raw material gas can also be supplementarily supplied to this part.
[0081] The C-doped raw material gas is supplied from a direction perpendicular to the upper surface of the wafer 40. Specifically, the C-doped raw material gas is supplied from a direction perpendicular to the Si-doped high concentration region 24 at the downstream side of the main raw material gas 220 with respect to the rotation center of the wafer 40. Thus, the C-doped raw material gas can be selectively supplied to the Si-doped high concentration region 24.
[0082] The concentration of Si mixed in the Si high concentration region 24 increases as it approaches the outer peripheral side. Therefore, it is preferred that the C-doped raw material gas is supplied to multiple radial positions in the Si high concentration region 24, and it is preferred that the supply amount of the C-doped raw material gas supplied to the multiple radial positions is controlled to increase as it approaches the outer peripheral side.
[0083] The growth conditions of the GaN layer 20 of the embodiment are the same as those of the comparison method except for the supply conditions of the C-doped raw material gas. The supply conditions of the C-doped raw material gas (supply position, supply amount, supply timing, etc. of the C-doped raw material gas) can be appropriately set through experimental research to compensate for the excess n-type carrier concentration caused by the mixing of Si. As a rough standard concept, it can be cited that the supply conditions of the C-doped raw material gas are set in a manner that the concentration of the mixed Si and the concentration of the added C are equal at each radial position. However, since it is not easy to determine to what extent the added C compensates for the n-type carriers, the concentration of the added C can be appropriately adjusted.
[0084] It should be noted that, compared with the comparative embodiment without adding C, the addition of C can provide an effect of compensating at least a part of the excess n-type carrier concentration. Therefore, it is not necessary to add C to completely compensate for the excess n-type carrier concentration.
[0085] For example, it is not necessary for the peripheral C addition concentration to be equal to (or higher than) the peripheral Si mixing concentration. Among them, the peripheral C addition concentration is preferably 0.5 times or more of the peripheral Si mixing concentration. It should be noted that in order to avoid the peripheral C addition concentration becoming excessive, the peripheral C addition concentration is preferably less than 2 times the peripheral Si mixing concentration.
[0086] The concentration of C mixed in by the Ga source gas, that is, the central C concentration CC0, is, for example, 2×10 15 cm -3 The central C concentration CC0 is preferably reduced as much as possible to be below the lower limit of the central Si concentration CSi0. The added C concentration is an excess amount exceeding the central C concentration CC0, and such an excess C concentration contributes to the effect of compensating for the excess amount of the n-type carrier concentration in the embodiment.
[0087] Figure 4 1 is a graph showing an example of the C concentration distribution of the upper surface 25 of the GaN layer 20 according to the embodiment. The horizontal axis represents the measurement position in the plane in mm units, and the vertical axis represents the measurement position in 10 15 cm -3 The unit represents the C concentration. The C concentration of each measurement point in the X direction is represented by a black circle, and the C concentration of each measurement point in the Y direction is represented by a hollow quadrilateral. The average C concentration is represented by a cross.
[0088] The center C concentration CC0 is 2.01×10 15 cm -3 In the Si high concentration region 24, the C concentration is higher than the central C concentration CC0, that is, C is added. In accordance with the fact that the concentration of Si mixed in the outer side is higher, C is added in such a way that the concentration of added C is higher in the outer side. The peripheral C concentration CC1 is 3.26×10 15 cm -3 The excess of the peripheral C concentration CC1 over the central C concentration CC0, that is, the peripheral C addition concentration is 1.25×10 15 cm -3 The peripheral C addition concentration was 1.25×10 15 cm -3 The peripheral Si mixing concentration is 1.64×10 15 cm -3 0.76 times of.
[0089] The following further describes the features of the embodiment related to the height direction (depth direction, thickness direction) of adding C. As a general tendency, the thicker the GaN layer 20, the greater the concentration of Si mixed in the GaN layer 20. This is because the longer the growth time of the GaN layer 20, the more Si-containing deposits 230 attached to the upper surface 213 of the susceptor edge become. Therefore, the C doping raw material gas can be supplied at the time when the growth thickness is reached to which the Si mixed becomes above the specified concentration.
[0090] Figure 5 1 is a timing diagram schematically showing the supply method of C doping source gas at a representative position of the periphery (radial position 10 mm from the edge). The horizontal axis represents the growth thickness of the GaN layer 20, and the vertical axis represents the supply amount of C doping source gas. When the Si doping concentration in the periphery reaches a predetermined concentration, for example, the above-mentioned doping reference value ΔSi (0.4×10 15 cm -3 ) when the growth thickness T1 of the GaN layer 20 is reached, the supply of C-doped raw material gas is started. After that, the peripheral Si mixing concentration increases until the final growth thickness T2 of the GaN layer 20 is reached. Therefore, it is preferred to increase the supply amount of C-doped raw material gas as the growth thickness increases to cope with the increase in the peripheral Si mixing concentration.
[0091] It should be noted that, on the central side closer to the representative position of the periphery, the mixed Si is less than that of the representative position of the periphery. Therefore, on the central side, the timing of starting the supply of the C-doped raw material gas can be delayed compared with the representative position of the periphery. In addition, on the peripheral side (edge side) closer to the representative position of the periphery, the mixed Si is more than that of the representative position of the periphery. Therefore, on the peripheral side (edge side), the timing of starting the supply of the C-doped raw material gas can be advanced compared with the representative position of the periphery. On the central side closer to the peripheral side (edge side) than the representative position of the periphery, the supply amount of the C-doped raw material gas can also be increased as the growth thickness becomes thicker to cope with the increase in the concentration of mixed Si.
[0092] Figure 6 1 is a schematic cross-sectional view of a GaN layer 20 of an exemplary embodiment. The region to which C-doped raw material gas is not supplied is a region 21 to which C is not added, and the region to which C-doped raw material gas is supplied is a region 22 to which C is added. The following is explained using a representative position of the periphery (a radial position 10 mm from the edge) as an example. The range of thickness T2 below the upper surface 25 of the GaN layer 20 is the region 22 to which C is added, and the range of thickness T1 below the lower end of the region 22 to which C is added is the region 21 to which C is not added.
[0093] In the C-added region 22, the C concentration of the upper surface 25 is the highest, and the C concentration decreases downward from the upper surface 25. In addition, the C concentration in the region 21 to which C is not added is lower than the C concentration of the upper surface 25. That is, in the GaN layer 20, at a predetermined depth position from the upper surface 25 at a representative position of the periphery (a radial position of 10 mm from the edge), there is a region where the C concentration is lower than the peripheral C concentration of the upper surface 25.
[0094] In addition, as described above, as a general tendency, the thicker the GaN layer 20, the greater the concentration of Si mixed in the GaN layer 20. In other words, as a general tendency, the lower the concentration of Si mixed in the GaN layer 20 is, the lower the concentration is. That is, in the GaN layer 20, at a depth position specified from the upper surface 25 at a representative position of the periphery (a radial position of 10 mm from the edge), there is a region where the Si concentration is lower than the peripheral Si concentration of the upper surface 25.
[0095] The following further describes the characteristics of the GaN layer 20 of the embodiment. The concentration of the mixed Si decreases monotonically from the outer peripheral side to the central side of the GaN layer 20. Therefore, the GaN layer 20 of the embodiment has the following characteristics: the intermediate Si concentration CSi2 at the radial position between the center and the periphery is higher than the central Si concentration CSi0, and lower than the peripheral Si concentration CSi1.
[0096] The intermediate Si concentration CSi2 is set to be, for example, the average Si concentration at a radial position 30 mm from the center. Figure 8 In the example shown, the intermediate Si concentration CSi2 (9.94×10 15 cm -3 ) than the central Si concentration CSi0(9.01×10 15 cm -3 ) is higher than the peripheral Si concentration CSi1 (10.65×10 15 cm -3 )Low.
[0097] In a manner corresponding to the concentration distribution shape of the mixed Si, the concentration of the added C is also preferably monotonically reduced from the outer peripheral side to the central side of the GaN layer 20. That is, the GaN layer 20 of the embodiment preferably has the following characteristics: the intermediate C concentration CC2 at the radial position between the center and the periphery is higher than the central C concentration CC0 and lower than the peripheral C concentration CC1.
[0098] The intermediate C concentration CC2 is set to be, for example, the average C concentration at a radial position of 30 mm from the center. Figure 4 In the example shown, the intermediate C concentration CC2 (2.73×10 15 cm -3) is higher than the central C concentration CC0 (2.01×10 15 cm -3 ), which is lower than the peripheral C concentration CC1 (3.26×10 15 cm -3 ).
[0099] <Preferred Mode of the Invention>
[0100] Preferred embodiments of the present invention are described below.
[0101] (Note 1)
[0102] A laminate substrate, characterized by comprising:
[0103] a base substrate; and
[0104] a gallium nitride layer epitaxially grown on the base substrate and composed of gallium nitride doped with silicon,
[0105] The gallium nitride layer has an upper surface with a radius of more than 50 mm,
[0106] The thickness of the gallium nitride layer is greater than 4 μm,
[0107] The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central silicon concentration at the center of the upper surface.
[0108] The central silicon concentration is 4×10 15 cm -3 More than and less than 2×10 16 cm -3 ,
[0109] The carbon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral carbon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central carbon concentration at a center of the upper surface.
[0110] (Note 2)
[0111] A stacked substrate according to Appendix 1, wherein in the gallium nitride layer, at a radial position of 10 mm from the edge of the upper surface and at a predetermined depth from the upper surface, there exists a region having a carbon concentration lower than the peripheral carbon concentration of the upper surface.
[0112] (Note 3)
[0113] A stacked substrate according to Note 1 or 2, wherein in the gallium nitride layer, at a radial position of 10 mm from the edge of the upper surface and at a predetermined depth from the upper surface, there exists a region where the silicon concentration is lower than the peripheral silicon concentration of the upper surface.
[0114] (Note 4)
[0115] The stacked substrate according to any one of Appendixes 1 to 3, wherein the silicon concentration of the upper surface of the gallium nitride layer has the following distribution: the intermediate silicon concentration at a radial position 30 mm away from the center of the upper surface is higher than the central silicon concentration and lower than the peripheral silicon concentration.
[0116] (Note 5)
[0117] The stacked substrate according to any one of Appendixes 1 to 4, wherein the carbon concentration of the upper surface of the gallium nitride layer has the following distribution: the intermediate carbon concentration at a radial position 30 mm from the center of the upper surface is higher than the central carbon concentration and lower than the peripheral carbon concentration.
Claims
1. A laminate substrate, It is characterized in that have: a base substrate; and a gallium nitride layer epitaxially grown on the base substrate and composed of gallium nitride doped with silicon, The gallium nitride layer has an upper surface with a radius of more than 50 mm, The thickness of the gallium nitride layer is greater than 4 μm. The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral silicon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central silicon concentration at the center of the upper surface. The central silicon concentration is 4×10 15 cm -3 More than and less than 2×10 16 cm -3 , The carbon concentration of the upper surface of the gallium nitride layer has a distribution in which a peripheral carbon concentration at a radial position 10 mm from an edge of the upper surface is high relative to a central carbon concentration at a center of the upper surface.
2. The laminate substrate according to claim 1, in, In the gallium nitride layer, at a radial position of 10 mm from the edge of the upper surface and at a predetermined depth from the upper surface, there exists a region having a carbon concentration lower than the carbon concentration in the periphery of the upper surface.
3. The laminate substrate according to claim 1 or 2, in, In the gallium nitride layer, at a radial position of 10 mm from the edge of the upper surface and at a predetermined depth from the upper surface, there exists a region having a silicon concentration lower than the silicon concentration in the periphery of the upper surface.
4. The laminate substrate according to claim 1 or 2, in, The silicon concentration of the upper surface of the gallium nitride layer has a distribution in which a middle silicon concentration at a radial position 30 mm from the center of the upper surface is higher than the central silicon concentration and lower than the peripheral silicon concentration.
5. The laminated substrate according to claim 1 or 2, in, The carbon concentration of the upper surface of the gallium nitride layer has a distribution in which an intermediate carbon concentration at a radial position 30 mm from the center of the upper surface is higher than the central carbon concentration and lower than the peripheral carbon concentration.