Preparation method and application of microgel nucleating agent modified polylactic acid composite fiber

By introducing a microgel nucleating agent into polylactic acid to form a three-dimensional network structure, it solves the problems of poor toughness and insufficient thermal stability of polylactic acid materials, improves the crystallinity and thermal stability of the fiber, and is suitable for a variety of application fields.

CN118773767AActive Publication Date: 2024-10-15QINGDAO UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410908562.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Traditional polylactic acid materials have poor toughness, low glass transition temperature, poor thermal stability and wear resistance, which limit their application in fields such as clothing, home textiles and automotive interiors.

Method used

By introducing a microgel nucleating agent into polylactic acid, a three-dimensional network structure is formed, which limits the free movement of PLA chain segments, improves elastic modulus and resistance to shear deformation, and allows chain sliding in the molten form to achieve nucleation and Physical cross-linking.

Benefits of technology

It significantly improves the crystallinity, glass transition temperature and strength of polylactic acid fiber, enhances thermal stability and heat curl resistance, and is suitable for clothing, home textiles, automobile interiors and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773767A_ABST
    Figure CN118773767A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a microgel nucleating agent modified polylactic acid composite fiber, and relates to the technical field of polylactic acid modification, and the microgel nucleating agent modified polylactic acid composite fiber comprises the following raw materials by weight: 90-95 parts of PLA resin; 1-5 parts of a multi-component epoxy monomer; 1-4 parts of a ring opening agent; and 0-5 parts of a functional auxiliary agent. The microgel nucleating agent is introduced into PLA through in-situ melt reaction, and the microgel nucleating agent can be used as a nucleating agent to improve the crystallization performance and can also be used as a physical cross-linking agent. By introducing the microgel nucleating agent, a three-dimensional network structure is generated in PLA, free movement of a PLA chain segment is limited, and the elastic modulus and shear deformation resistance of a system are improved; meanwhile, a physical interpenetrating cross-linked network allows a PLA chain to have a certain degree of sliding freedom in a molten state, so that the fluidity during melt spinning is ensured; the preparation process of the microgel nucleating agent in the method does not need an independent synthesis step, the microgel nucleating agent can be added together with an auxiliary agent in the melt blending process, and no additional technological process is added.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polylactic acid modification, and in particular to a preparation method and application of polylactic acid composite fibers modified with a microgel nucleating agent. Background Art

[0002] Polylactic acid (PLA) is a biodegradable polymer made from renewable resources such as corn or sugarcane, with good biocompatibility and environmental friendliness. However, traditional PLA materials have defects such as poor toughness, low glass transition temperature, poor thermal stability and wear resistance during application, which seriously limit their commercial application.

[0003] Due to the irregularity of the PLA molecular chain, the carbonyl group on the chain forms intermolecular or intramolecular hydrogen bonds with the hydrogen on the adjacent molecular chain, which leads to poor mobility of the PLA molecular chain and affects the diffusion rate of the molecular chain to the lattice. Therefore, the regular arrangement of the molecular chain is seriously affected during the melt cooling process, so that the heat deformation temperature (HDT) is only 55-65℃. In addition, PLA also has problems such as difficulty in homogeneous nucleation, large spherulite size, and slow crystallization rate during the melt spinning process, which leads to low mechanical strength and poor heat resistance of PLA fibers, which seriously limits its application in the fields of clothing, home textiles, and automotive interiors. With the increasing attention paid by academia and industry to heat-resistant PLA materials, research on heat-resistant PLA materials at home and abroad has become more and more in-depth. At present, the main methods to improve the heat resistance of PLA materials are: blending modification, chain structure modification, and crystallization modification. Summary of the invention

[0004] In order to solve the above technical problems, the present invention discloses a preparation method and application of a microgel nucleating agent modified polylactic acid composite fiber. The method introduces a microgel nucleating agent into PLA through an in-situ melt reaction, which can act as a nucleating agent to improve the crystallization performance and a physical crosslinking agent. The introduction of the microgel nucleating agent generates a three-dimensional network structure inside the PLA, restricts the free movement of the PLA chain segments, and improves the elastic modulus and shear deformation resistance of the system; at the same time, the physical interpenetrating crosslinking network allows the PLA chain to have a certain degree of sliding freedom in the molten state, ensuring the fluidity during melt spinning.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A microgel nucleating agent modified polylactic acid composite fiber, characterized by comprising the following raw materials in parts by weight:

[0007] 90-95 parts of PLA resin;

[0008] 1-5 parts of polyvalent epoxy monomer;

[0009] 1-4 parts of ring-opening agent;

[0010] Functional additives 0-5 parts.

[0011] Furthermore, the polycyclic epoxy monomer is selected from one of epoxidized soybean oil, epoxidized castor oil, epoxidized palm oil, epoxidized rapeseed oil, and catechol polycyclic epoxy.

[0012] Furthermore, the ring-opening agent is selected from one of tannic acid, cardanol, dopamine oligomers, and gallic acid modified substances.

[0013] Furthermore, the molar ratio of the polyvalent epoxy monomer to the ring-opening agent is 0.5:9.5-9.5:0.5.

[0014] Furthermore, the functional additives include antioxidants, antibacterial agents, plasticizers and whitening agents.

[0015] The present invention also discloses a method for preparing a microgel nucleating agent modified polylactic acid composite fiber, the specific process of which is as follows:

[0016] a. PLA resin, multi-epoxy monomer, ring-opening agent and additives in a certain ratio are uniformly mixed, added into an internal mixer for melt blending, the melt temperature is controlled at 170-230°C, the blending time is 3-10min, and the rotor speed is 20-120r / min to obtain a masterbatch; the masterbatch is crushed and then sent into a micro-spinning machine for melt spinning, and cooled in air to obtain a microgel nucleating agent modified polylactic acid composite fiber spun yarn;

[0017] Or b. PLA resin, multi-epoxy monomer, ring-opening agent and auxiliary agent in a certain ratio are mixed evenly, and added into a twin-screw extruder at a uniform speed. The temperature of the extruder is set to 140-230° C. and the screw speed is set to 15-100 r / min to obtain a masterbatch; after the masterbatch is granulated, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain microgel nucleating agent modified polylactic acid composite fiber spinning chips.

[0018] Furthermore, in a and b, the melt blending equipment is selected from internal mixer, single screw extruder, twin screw extruder, three screw extruder, four screw extruder.

[0019] Furthermore, in a and b, the melt spinning conditions are: spinning temperature is 160-240°C, hot drawing temperature is 80-120°C, heat setting temperature is 60-120°C, and drawing ratio is 1.5, 2.0, 2.5, 3.0.

[0020] Furthermore, the microgel nucleating agent modified polylactic acid composite fiber has a strength greater than 2.5 cN / dtex, a crystallinity of 50%, and a glass transition temperature of 85°C; there is no obvious thermal curling in boiling water or 100°C hot air, and the thermal shrinkage rate is 3-10%.

[0021] The invention also discloses the application of the microgel nucleating agent modified polylactic acid composite fiber in clothing, home textiles and automobile interior decoration.

[0022] The beneficial effects of the present invention are as follows, compared with the prior art:

[0023] This method introduces microgel nucleating agents into PLA through in-situ melt reaction, which can act as nucleating agents to improve crystallization performance and physical crosslinking agents. The introduction of microgel nucleating agents generates a three-dimensional network structure inside PLA, restricts the free movement of PLA segments, and improves the elastic modulus and shear deformation resistance of the system; at the same time, the physical interpenetrating crosslinking network allows PLA chains to have a certain degree of sliding freedom in the molten state, ensuring fluidity during melt spinning.

[0024] In this method, the preparation process of the microgel nucleating agent does not require a separate synthesis step, and can be added together with auxiliary agents (such as antibacterial agents, antioxidants, flame retardants) during the melt blending process without adding additional process steps.

[0025] A one-step spinning method can also be used to directly use the microgel-containing PLA melt for melt spinning by controlling the screw length, reaction temperature, and residence time.

[0026] The system of microgel nucleating agent generated by in-situ melt reaction is not only suitable for PLA fiber, but also suitable for the preparation of PLA-based composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the DSC curve structure of pure PLA (6201D) and the prepared microgel nucleating agent modified polylactic acid composite fiber in Example 2 of the present invention;

[0028] Figure 2 is the loss factor of the PLA characterized by DMA and the prepared microgel nucleating agent modified polylactic acid composite fiber in Example 2 of the present invention;

[0029] Figure 3 This is a physical picture of the thermal shrinkage of pure PLA (LX175) and the prepared microgel nucleating agent modified polylactic acid composite fiber at 100°C in Example 4 of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The present invention introduces a microgel nucleating agent into PLA through an in-situ melt reaction, and the microgel nucleating agent can improve the crystallinity of PLA fibers and increase the glass transition temperature. At the same time, branched PLA or free radical cross-linked PLA can also increase its crystallinity, glass transition temperature and strength, but the processing performance will be reduced. The present invention aims to provide a method for preparing a microgel nucleating agent that can have a nucleating agent effect and can construct a physical cross-linking network inside PLA, conveniently and efficiently modify PLA, and improve the performance of PLA fibers.

[0032] Example 1

[0033] A method for preparing a microgel nucleating agent modified polylactic acid composite fiber, the specific process is:

[0034] (1) 50 g of spinning-grade PLA (6201D, Natureworks), 3.5 g of epoxidized soybean oil, and 1.5 g of tannic acid were mixed evenly and added to an internal mixer for melt blending. The melt temperature was controlled at 200° C., the blending time was 6 min, and the rotor speed was 80 r / min to obtain a masterbatch.

[0035] (2) After the masterbatch is crushed, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain the microgel nucleating agent modified polylactic acid composite fiber spun fibers (PLA composite fiber 1).

[0036] The melt spinning conditions are as follows: spinning temperature is 205°C, heat drawing temperature is 110°C, heat setting temperature is 90°C, drawing ratio is 2.5, and drawing rate is 100 m / min.

[0037] Example 2

[0038] A method for preparing a microgel nucleating agent modified polylactic acid composite fiber, the specific process is:

[0039] (1) 50 g of spinning-grade PLA (6201D, Natureworks), 3.0 g of epoxidized soybean oil, and 2.0 g of tannic acid were mixed uniformly and added into a twin-screw extruder at a uniform speed. The temperatures of each section were 140° C., 160° C., 175° C., 185° C., and 200° C., respectively, and the screw speed was set to 60 r / min to obtain a masterbatch.

[0040] (2) After the masterbatch is granulated, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain microgel nucleating agent modified polylactic acid composite fiber spinning chips (PLA composite fiber 2).

[0041] The melt spinning conditions are as follows: spinning temperature is 210° C., heat drawing temperature is 115° C., heat setting temperature is 95° C., drawing ratio is 2.5, and drawing rate is 150 m / min.

[0042] When the draw ratio is 2, the thermal properties of pure PLA and PLA composite fiber 2 are shown in Table 1. After drawing, the pure PLA fiber and PLA composite fiber 2 have no obvious glass transition temperature and cold crystallization temperature. The melting temperature T m1 and T m2 Compared with pure PLA fiber, the temperature is 3.5℃ and 5.7℃ higher, and the crystallinity is more than 45%.

[0043] Table 1

[0044] sample <![CDATA[T g (℃)]]> <![CDATA[T c (℃)]]> <![CDATA[T m1 (℃)]]> <![CDATA[T m2 (℃)]]> <![CDATA[ΔH c (J / g)]]> <![CDATA[ΔH m (J / g)]]> <![CDATA[χ m (%)]]> Pure PLA(6201D) - - 152.8 141.7 - 38.3 40.0 PLA composite fiber 2 - - 156.3 147.4 - 37.8 46.2

[0045] The loss factor (Tanδ) measured by DMA showed that the Tg of PLA composite fiber 2 (86.9℃) was 8.5℃ higher than that of pure PLA (78.4℃). Figure 2 ).

[0046] Example 3

[0047] A method for preparing a microgel nucleating agent modified polylactic acid composite fiber, the specific process is:

[0048] (1) 50 g of spinning-grade PLA (6201D, Natureworks), 3.5 g of epoxidized soybean oil, 1.5 g of tannic acid, 0.25 g of antioxidant, 0.50 g of plasticizer, and 0.1 g of brightener were mixed uniformly, added to an internal mixer for melt blending, and the melt temperature was controlled at 200° C. to obtain a masterbatch.

[0049] (2) After the masterbatch is crushed, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain the microgel nucleating agent modified polylactic acid composite fiber spun fibers (PLA composite fiber 3).

[0050] The melt spinning conditions are as follows: spinning temperature is 210° C., heat drawing temperature is 110° C., heat setting temperature is 95° C., drawing ratio is 2.0, and drawing rate is 100 m / min.

[0051] Example 4

[0052] A method for preparing a microgel nucleating agent modified polylactic acid composite fiber, the specific process is:

[0053] (1) 50 g spinning grade PLA (LX175, Total), 3.0 g epoxy soybean oil, 2.0 g tannic acid, 0.25 g antioxidant, 0.50 g plasticizer, and 0.1 g antibacterial agent were mixed evenly and added into a twin-screw extruder at a uniform speed. The temperatures of each section were 150°C, 170°C, 190°C, 200°C, and 210°C, respectively, and the screw speed was set to 60 r / min to obtain a masterbatch.

[0054] (2) After the masterbatch is granulated, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain microgel nucleating agent modified polylactic acid composite fiber spinning chips (PLA composite fiber 4).

[0055] The melt spinning conditions are as follows: spinning temperature is 210° C., heat drawing temperature is 115° C., heat setting temperature is 95° C., drawing ratio is 2.5, and drawing rate is 150 m / min.

[0056] The results of the 100℃ air thermal stability test are as follows: Figure 3 As shown in Table 2, it is shown that the pure PLA (6201D) and the PLA (LX175) spun filaments of Example 4 both curl in hot air at 100°C, with a thermal shrinkage of more than 50%. After hot drawing, the pure PLA fiber still curls, with a thermal shrinkage of 12.6%. In contrast, the composite fiber of Example 4 does not curl, with a thermal shrinkage of 7.5%, indicating that microgel nucleation can greatly improve the thermal stability of the PLA composite fiber.

[0057] Table 2

[0058] sample curly Shrinkage / % PLA(6201D virgin silk yes 54.0 Pure PLA yes 12.6 PLA(LX175) virgin silk yes 53.0 PLA composite fiber 4 no 7.5

[0059] Example 5

[0060] A method for preparing a microgel nucleating agent modified polylactic acid composite fiber, the specific process is:

[0061] (1) 50 g spinning grade PLA (6201D, Natureworks), 0.5 g tetraepoxy monomer, 0.5 g tannic acid, 0.25 g antioxidant, 0.1 g antibacterial agent, and 0.1 g whitening agent were mixed uniformly and added into a twin-screw extruder at a uniform speed. The temperatures of each section were 150° C., 170° C., 190° C., 200° C., and 210° C., respectively, and the screw speed was set to 60 r / min to obtain a masterbatch.

[0062] (2) After the masterbatch is granulated, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain microgel nucleating agent modified polylactic acid composite fiber spinning chips (PLA composite fiber 5).

[0063] The melt spinning conditions are as follows: spinning temperature is 210°C, heat drawing temperature is 115°C, heat setting temperature is 100°C, drawing ratio is 2.5, and drawing rate is 130 m / min.

[0064] The mechanical properties of the microgel nucleating agent modified polylactic acid composite fibers prepared in the above examples were tested, and the results are shown in Table 3 below. The strength of the composite fibers after heat drawing is greatly improved compared to that of the spun fibers.

[0065] Table 3

[0066] sample Primary silk strength (cN / dtex) Strength after hot drawing (cN / dtex) Pure PLA(6201D) 0.80±0.10 2.75±0.20 PLA composite fiber 1 0.82±0.07 2.63±0.12 PLA composite fiber 2 1.00±0.09 2.43±0.18 PLA composite fiber 3 1.03±0.03 2.31±0.08 PLA composite fiber 4 1.01±0.06 2.45±0.11 PLA composite fiber 5 1.54±0.06 3.10±0.22

[0067] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A microgel nucleating agent modified polylactic acid composite fiber, characterized in that: The invention comprises the following raw materials in parts by weight: 90-95 parts of PLA resin; 1-5 parts of polyvalent epoxy monomer; 1-4 parts of ring-opening agent; Functional additives 0-5 parts.

2. The microgel nucleating agent modified polylactic acid composite fiber according to claim 1, characterized in that: The polycyclic epoxy monomer is selected from one of epoxidized soybean oil, epoxidized castor oil, epoxidized palm oil, epoxidized rapeseed oil and catechol polycyclic epoxy.

3. A microgel nucleating agent modified polylactic acid fiber as claimed in claim 2, characterized in that: The ring-opening agent is selected from one of tannic acid, cardanol, dopamine oligomers, and gallic acid modifiers.

4. A microgel nucleating agent modified polylactic acid composite fiber as claimed in claim 3, characterized in that: The molar ratio of the polyvalent epoxy monomer to the ring-opening agent is 0.5:9.5-9.5:0.

5.

5. The microgel nucleating agent modified polylactic acid composite fiber according to claim 4, characterized in that: The functional additives include antioxidants, antibacterial agents, plasticizers and whitening agents.

6. The method for preparing the microgel nucleating agent modified polylactic acid composite fiber according to claim 5, characterized in that: The specific process is as follows: a. PLA resin, multi-epoxy monomer, ring-opening agent and additives in a certain ratio are uniformly mixed, added into an internal mixer for melt blending, the melt temperature is controlled at 170-230°C, the blending time is 3-10min, and the rotor speed is 20-120r / min to obtain a masterbatch; the masterbatch is crushed and then sent into a micro-spinning machine for melt spinning, and cooled in air to obtain a microgel nucleating agent modified polylactic acid composite fiber spun yarn; Or b. PLA resin, multi-epoxy monomer, ring-opening agent and auxiliary agent in a certain ratio are mixed evenly, and added into a twin-screw extruder at a uniform speed. The temperature of the extruder is set to 140-240°C and the screw speed is set to 20-200r / min to obtain a masterbatch; after the masterbatch is granulated, it is sent to a micro-spinning machine for melt spinning and cooled in air to obtain microgel nucleating agent modified polylactic acid composite fiber spinning chips.

7. The method for preparing the microgel nucleating agent modified polylactic acid composite fiber according to claim 6, characterized in that: In a and b, the melt blending equipment is selected from internal mixer, single screw extruder, twin screw extruder, three screw extruder, four screw extruder.

8. The method for preparing the microgel nucleating agent modified polylactic acid composite fiber according to claim 7, characterized in that: In a and b, the melt spinning conditions are: spinning temperature of 160-240°C, hot drawing temperature of 80-120°C, heat setting temperature of 60-120°C, drawing ratio of 1.5, 2.0, 2.5, 3.0, and drawing rate of 100-2000 cm / min.

9. The method for preparing the microgel nucleating agent modified polylactic acid composite fiber according to claim 8, characterized in that: The strength of the microgel nucleating agent modified polylactic acid composite fiber is greater than 2.5 cN / dtex, the crystallinity is more than 45%, and the glass transition temperature is 86.9°C; there is no obvious thermal curling phenomenon in boiling water or 100°C hot air, and the thermal shrinkage rate is 3-10%.

10. Application of the polylactic acid composite fiber modified by the microgel nucleating agent as claimed in claim 1 in clothing, home textiles and automobile interior decoration.

Citation Information

Patent Citations

  • Polylactic acid fiber with high hydrolytic resistance performance

    CN101748509A

  • High-hydrolysis resistance polylactic acid fiber and preparation method thereof

    CN102094257A

  • A method for preparing highly efficient hydrolysis-resistant flexible PLA fibers

    CN102286801A

  • Highly-resistance hydrolysis polylactic acid fiber suitable for fishing net and garment and preparation method thereof

    CN105133076A

  • Partially crosslinked epoxy natural rubber modified polylactic acid and preparation method thereof

    CN113698748A