Production method of fiber blended composite fabric

By using the mixing process of mulberry fiber, marine regenerated fiber and flame-retardant fiber in the fiber blended composite fabric, the problem of the lack of special functions of traditional fabrics is solved, the flame-retardant performance and comfort of the fabric are improved, and it is suitable for a variety of applications occasion.

CN118773798AInactive Publication Date: 2024-10-15YANCHENG INST OF IND TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972384.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the absence of special fibers, traditional fiber blended composite fabrics cannot achieve special functions such as waterproofing, flame retardancy, and antibacterial, which limits the application fields and performance of the fabrics.

Method used

Mulberry fiber, marine recycled fiber and flame-retardant fiber are mixed according to the designed proportion, and processed through carding, drawing, spinning and weaving processes to form a composite fabric to enhance its flame-retardant performance and comfort.

Benefits of technology

It improves the flame retardant performance, antibacterial and anti-odor properties of the fabric, provides a comfortable, environmentally friendly and safe wearing experience, and expands the application scope of the fabric.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of fiber blended composite fabric production, and discloses a fiber blended composite fabric production method which comprises the following steps: step 1, raw material selection; 2, uniformly mixing the raw materials according to a design proportion; 3, further carding the mixed fibers through a carding machine; 4, drawing the mixed fiber strips through a drawing frame; 5, the drawn fibers are made into roving through a roving frame; sixthly, the rough yarn is spun and formed through a spinning frame, and yarn of the needed specification is obtained; and 7, drafting and weaving the yarns on a weaving machine. According to the blended composite fabric, 30%-40% of the mulberry fibers, 30%-40% of the marine regenerated fibers and 10%-20% of the flame-retardant fibers are mixed together to be further carded, drawing is carried out, spun yarn forming is carried out, the yarn of the needed specification is obtained, the blended composite fabric can provide comfortable, environment-friendly and safe wearing experience, and the blended composite fabric is suitable for being used in the field of textile fabrics. The garment is suitable for garment manufacturing in various occasions and seasons.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber blended composite fabric production, in particular to a fiber blended composite fabric production method. Background Art

[0002] Composite fabric is a new type of fabric formed by combining two or more fibers or fabrics of different materials through a composite process. This type of fabric usually combines the advantages of various raw materials to obtain a variety of properties and characteristics. The manufacturing process of composite fabrics usually involves stacking different materials together and then firmly connecting them together through pressing, bonding or fusing. Fiber blended composite fabric refers to mixing two or more different types of fibers (such as natural fibers, synthetic fibers, etc.) and compounding them through a specific process method to form a new type of fabric. This fabric combines the advantages of different types of fibers to achieve better comprehensive performance. Fiber blended composite fabrics usually involve mixing, spinning, weaving or non-woven processing of different types of fibers, and firmly combining the fibers together through coating, bonding, melting and other methods. This composite fabric can have a sense of hierarchy in structure, or it can be a uniform mixture of fibers. Different production methods are selected according to different design requirements and application scenarios.

[0003] At present, in the production process of fiber blended composite fabrics, the fiber materials are mixed evenly in a certain proportion before production. However, due to the lack of special fibers added, the fiber blended composite fabrics produced by the traditional production method cannot achieve special functions such as waterproof, flame retardant, and antibacterial when used, which limits the application field and performance of the fabrics. Therefore, fiber blended composite fabrics without adding mulberry fiber, marine recycled fiber and flame retardant fiber may have certain defects in functionality, environmental protection, comfort, safety, durability and other aspects, which will limit the application scope and performance of the fabrics. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for producing a fiber blended composite fabric, which solves the problem that the fiber blended composite fabric produced by the traditional production method cannot achieve special functions such as waterproofing, flame retardancy, and antibacterial when used due to the lack of special fibers, thus limiting the application field and performance of the fabric.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for producing a fiber blended composite fabric comprises the following steps:

[0006] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0007] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0008] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0009] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0010] Step 5, the drawn fibers are made into rovings by a roving machine;

[0011] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0012] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0013] Preferably, in step 2, the mulberry fiber may account for 30%-40% of the total proportion, the marine regenerated fiber may account for 30%-40% of the total proportion, and the flame retardant fiber may account for 10%-20% of the total proportion.

[0014] Preferably, in step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0015] Preferably, in step 4, the spacing between the drawing frame rollers is 0.1 mm-0.3 mm, and the rotation speed of the drawing frame rollers is 100-200 RPM (revolutions per minute).

[0016] Preferably, in step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0017] Preferably, in step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0018] Preferably, in step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0019] Preferably, in step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0020] The present invention provides a method for producing a fiber blended composite fabric. It has the following beneficial effects:

[0021] The present invention improves the comfortable touch and wearing experience of the fabric by using mulberry fiber to have a soft feel and a comfortable wearing feel. The marine regenerated fiber has antibacterial and deodorizing properties, which can effectively reduce bacterial growth and keep the fabric fresh. The addition of flame retardant fiber enhances the flame retardant performance of the fabric and improves the safety of the fabric in accidental situations such as fire. It can have a soft feel and a comfortable wearing feel and has antibacterial and deodorizing properties while protecting the safety of the wearer. Therefore, the blended composite fabric can provide a comfortable, environmentally friendly, safe and functional wearing experience, and is suitable for clothing manufacturing in various occasions and seasons. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0025] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0026] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0027] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0028] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0029] Step 5, the drawn fibers are made into rovings by a roving machine;

[0030] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0031] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0032] In step 2, the mulberry fiber may account for 35% of the total proportion, the marine regenerated fiber may account for 35% of the total proportion, and the flame retardant fiber may account for 15% of the total proportion.

[0033] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0034] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0035] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0036] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0037] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0038] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0039] Embodiment 2:

[0040] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0041] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0042] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0043] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0044] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0045] Step 5, the drawn fibers are made into rovings by a roving machine;

[0046] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0047] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0048] In step 2, the mulberry fiber may account for 30% of the total proportion, the marine regenerated fiber may account for 40% of the total proportion, and the flame retardant fiber may account for 15% of the total proportion.

[0049] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0050] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0051] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0052] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0053] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0054] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0055] Embodiment three:

[0056] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0057] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0058] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0059] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0060] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0061] Step 5, the drawn fibers are made into rovings by a roving machine;

[0062] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0063] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0064] In step 2, the mulberry fiber may account for 40% of the total proportion, the marine regenerated fiber may account for 30% of the total proportion, and the flame retardant fiber may account for 15% of the total proportion.

[0065] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0066] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0067] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0068] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0069] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0070] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0071] Embodiment 4:

[0072] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0073] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0074] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0075] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0076] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0077] Step 5, the drawn fibers are made into rovings by a roving machine;

[0078] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0079] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0080] In step 2, the mulberry fiber may account for 30% of the total proportion, the marine regenerated fiber may account for 30% of the total proportion, and the flame retardant fiber may account for 20% of the total proportion.

[0081] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0082] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0083] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0084] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0085] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0086] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0087] Embodiment five:

[0088] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0089] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0090] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0091] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0092] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0093] Step 5, the drawn fibers are made into rovings by a roving machine;

[0094] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0095] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0096] In step 2, the mulberry fiber may account for 40% of the total proportion, the marine regenerated fiber may account for 40% of the total proportion, and the flame retardant fiber may account for 10% of the total proportion.

[0097] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0098] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0099] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0100] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0101] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0102] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0103] Embodiment six:

[0104] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0105] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0106] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0107] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0108] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0109] Step 5, the drawn fibers are made into rovings by a roving machine;

[0110] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0111] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0112] In step 2, the mulberry fiber may account for 38% of the total proportion, the marine regenerated fiber may account for 42% of the total proportion, and the flame retardant fiber may account for 10% of the total proportion.

[0113] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0114] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0115] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0116] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0117] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0118] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0119] Embodiment seven:

[0120] The embodiment of the present invention provides a method for producing a fiber blended composite fabric, comprising the following steps:

[0121] Step 1: Raw material selection. Mulberry fiber: select mulberry fiber with good spinning performance and strength, which is usually extracted from mulberry leaves or mulberry bark after preliminary processing. Marine recycled fiber: select fiber materials recycled from the ocean, such as marine plastic waste or fibers extracted from other renewable resources. Flame retardant fiber: select fibers with flame retardant properties, such as flame retardant polyester fiber, flame retardant polyamide fiber, etc., to ensure that the fabric has flame retardant properties.

[0122] Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion;

[0123] Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers;

[0124] Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing;

[0125] Step 5, the drawn fibers are made into rovings by a roving machine;

[0126] Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications;

[0127] Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

[0128] In step 2, the mulberry fiber may account for 33% of the total proportion, the marine regenerated fiber may account for 44% of the total proportion, and the flame retardant fiber may account for 10% of the total proportion.

[0129] In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM (revolutions per minute).

[0130] In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM (revolutions per minute).

[0131] In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM (revolutions per minute).

[0132] In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

[0133] In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

[0134] In step six, the twist of the yarn is between 300-600 TPM (twists per minute).

[0135] Example Heat resistance Softness Embodiment 1 middle middle Embodiment 2 middle Low Embodiment 3 middle high Embodiment 4 high Low Embodiment 5 Low high Embodiment 6 Low middle Embodiment 7 Low middle

[0136] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for producing a fiber blended composite fabric, characterized in that: The following steps are involved: Step 1, raw material selection: select mulberry fiber with good spinning performance and strength, fiber extracted from mulberry leaves or mulberry bark after preliminary processing, fiber materials recycled from the ocean, fiber extracted from marine plastic waste or other renewable resources, and fiber with flame retardant properties, flame retardant polyester fiber, flame retardant polyamide fiber, to ensure that the fabric has flame retardant properties; Step 2, mixing mulberry fiber, marine recycled fiber and flame retardant fiber evenly according to the designed proportion; Step 3: The mixed fibers are further combed by a combing machine to enhance the parallelism and mixing uniformity of the fibers; Step 4, drawing the mixed fiber strips through a drawing frame to increase the uniformity of the drawing; Step 5, the drawn fibers are made into rovings by a roving machine; Step 6: the roving is spun through a spinning frame to obtain yarn of required specifications; Step seven: The yarn is threaded and woven on the loom according to the design requirements to form the basic cloth structure.

2. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step 2, the mulberry fiber can account for 30%-40% of the total proportion, the marine regenerated fiber can account for 30%-40% of the total proportion, and the flame retardant fiber can account for 10%-20% of the total proportion.

3. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step three, the spacing of the combing rollers is set to 0.1 mm-0.3 mm, and the speed of the combing rollers is set to 100-200 RPM.

4. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step 4, the spacing between the rollers of the drawing frame is 0.1 mm-0.3 mm, and the rotation speed of the rollers of the drawing frame is 100-200 RPM.

5. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step five, the spacing between the spinning rollers is between 1 mm and 3 mm, and the rotation speed of the spinning machine is between 300 and 800 RPM.

6. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step six, the spacing between the spinning rollers is between 0.1 mm and 0.5 mm, and the rotation speed of the spinning machine is between 800 and 1500 RPM.

7. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step six, the fineness of the yarn is between Ne20 / 1 and Ne120 / 1.

8. The method for producing a fiber blended composite fabric according to claim 1, characterized in that: In step six, the twist of the yarn is between 300-600 TPM.