Printing and dyeing method for alkali-soluble silk fabric

By utilizing the dissolution of alkali-soluble silk yarn and the stability of T400 fiber in alkali-soluble silk fabrics, combined with the different dissolution characteristics of viscose fiber and flax fiber, micro-voids and micro-void strips are formed, which solves the problem of fabrics in the existing technology. The problem of insufficient air permeability has been solved, and an efficient printing and dyeing process has been achieved and the air permeability of the fabric has been improved.

CN118773931APending Publication Date: 2024-10-15SUZHOU XINDA PRINTING & DYEING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028670.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing woven fabrics need to be physically punched and hollowed out after printing and dyeing. The process is cumbersome and consumes a lot of energy, resulting in insufficient breathability.

Method used

A printing and dyeing method for alkali-soluble silk fabrics is adopted. By spinning alkali-soluble silk fiber and T400 fiber, the alkali-soluble silk yarn is dissolved in an alkali solution after weaving, and the different dissolutions of viscose fiber and flax fiber are utilized. Characteristics, forming micro-voids and micro-void strips to improve the breathability of the fabric.

Benefits of technology

It improves the breathability of printed and dyed fabrics, simplifies the process, reduces energy consumption, and ensures that the structural strength and breathability of the fabric exist at the same time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773931A_ABST
    Figure CN118773931A_ABST
Patent Text Reader

Abstract

The invention discloses a printing and dyeing method for alkali-soluble silk fabric, which comprises the following steps: weaving alkali-soluble silk and T400 fiber by utilizing the characteristic that the alkali-soluble silk can be dissolved in alkali liquor, and dissolving the alkali-soluble silk on the manufactured fabric by utilizing the alkali liquor, so that the fabric is provided with micro-pores and micro-strips, the air permeability can be improved, and the alkali-soluble silk fabric can be dyed and dyed. The printing and dyeing efficiency in the printing and dyeing process is improved, and the defect that in the prior art, printed and dyed fabric is insufficient in breathability in the preparation process is overcome; the linen yarns and the T400 yarns in the warp yarns are alternately arranged, the viscose yarns are uniformly arranged between the linen yarns and the T400 yarns, the weft weaving frequencies of the viscose yarns, the linen yarns and the T400 yarns in the weft yarns are consistent, and the viscose yarns, the linen yarns and the T400 yarns are sequentially woven according to a fixed sequence, so that the air permeability of a viscose yarn dissolving area in the weaving process is improved; the air permeability and the structural strength of the fabric can exist at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabric preparation, in particular to a printing and dyeing method for alkali-soluble silk fabric. Background Art

[0002] For the original woven products with micro holes and micro stripes, the products must be physically punched and processed after dyeing, which has the problems of complicated procedures and huge energy consumption.

[0003] Therefore, it is necessary to improve the printing and dyeing fabrics in the prior art. Summary of the invention

[0004] The invention overcomes the shortcomings of the prior art and provides a printing and dyeing method for alkali-soluble silk fabrics, aiming to solve the defect of insufficient air permeability of the printed and dyed fabrics in the prior art during the preparation process.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a printing and dyeing method for alkali-soluble silk fabrics, comprising the following steps:

[0006] S1: spinning the alkali-soluble silk fiber and the T400 fiber separately to obtain the alkali-soluble silk yarn and the T400 yarn;

[0007] S2: weaving the alkali-soluble silk yarn and the T400 yarn, wherein both the warp yarn and the weft yarn contain the alkali-soluble silk yarn and the T400 yarn, to obtain an alkali-soluble silk coarse fabric;

[0008] S3: soaking the alkali-soluble silk coarse fabric in an alkali solution, dissolving the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric, taking out the alkali-soluble silk coarse fabric, washing and drying;

[0009] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0010] In a preferred embodiment of the present invention, the spinning treatment method of the alkali-soluble silk fiber in S1 is one of air-jet spinning and ring spinning, and the spinning treatment method of the T400 fiber is water-jet spinning.

[0011] In a preferred embodiment of the present invention, the raw materials of the alkali-soluble silk fiber in S1 include viscose fiber and flax fiber, and the viscose fiber and flax fiber exist in different fibers respectively, and viscose yarn and flax yarn are respectively prepared.

[0012] In a preferred embodiment of the present invention, the fineness of the viscose fiber and the flax fiber in S1 is 1.2-1.8 dtex and 1.5-2.5 dtex respectively, and the fineness of the T400 fiber is 1.9-2.8 dtex.

[0013] In a preferred embodiment of the present invention, when weaving is performed in S2, T400 yarns and linen yarns are arranged between adjacent viscose yarns in the warp yarns, the arrangement order of the viscose yarns, T400 yarns and linen yarns is fixed, and the total number of T400 yarns and linen yarns between every two adjacent viscose yarns is the same.

[0014] In a preferred embodiment of the present invention, when weaving in S2, the ratio of the number of T400 yarns between every two adjacent viscose yarns on the warp yarn to the number of linen yarns is 1:1, and the T400 yarns and linen yarns between every two adjacent viscose yarns are arranged alternately, and the ratio of the number of viscose yarns to the number of linen yarns on the warp yarn is 1:2-4.

[0015] In a preferred embodiment of the present invention, during weaving in S2, the viscose yarn, linen yarn and T400 yarn in the weft yarn are arranged in a 1:1:1 interval sequence.

[0016] In a preferred embodiment of the present invention, the main component of the alkaline solution in S3 can be one or more of sodium hydroxide and sodium bicarbonate.

[0017] In a preferred embodiment of the present invention, the concentrations of sodium hydroxide and sodium bicarbonate in the alkaline solution in S3 are both 0.0001 mol / L, and the soaking time is 40 min-60 min.

[0018] In a preferred embodiment of the present invention, the drying temperature in S3 is 90-120° C., and the drying time is 1 h-2 h.

[0019] The present invention solves the defects existing in the background technology and has the following beneficial effects:

[0020] (1) The present invention provides a printing and dyeing method for alkali-soluble silk fabrics. The alkali-soluble silk is woven with T400 fiber by utilizing the characteristic that the alkali-soluble silk can be dissolved in alkali solution, and the alkali-soluble silk on the manufactured fabric is dissolved by alkali solution, so that the fabric has micro-pores and micro-strips. Compared with the printing and dyeing fabrics in the prior art, the air permeability can be improved, so that the printing and dyeing efficiency in the printing and dyeing process is improved, and the defect of insufficient air permeability of the printing and dyeing fabrics in the prior art during the preparation process is solved.

[0021] (2) In the present invention, the alkali-soluble silk is made of viscose fiber and flax fiber. During the immersion in alkali solution, the yarn made of viscose fiber is dissolved, and the yarn made of flax fiber is etched, so that while ensuring the structural strength of the fabric, different degrees of dissolution results appear on the fabric. Compared with the prior art, different dissolution results can be utilized to improve the air permeability of the fabric from multiple aspects.

[0022] (3) In the present invention, the linen yarn and the T400 yarn in the warp are arranged alternately, the viscose yarn is evenly arranged between the linen yarn and the T400 yarn, and the weft yarns of the viscose yarn, the linen yarn and the T400 yarn have the same weft weaving frequency and are woven in a fixed order, so that the air permeability of the viscose yarn dissolving area during the weaving process is improved. Compared with the prior art, the air permeability and structural strength of the fabric can be achieved at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 It is a method step diagram of a preferred embodiment of the present invention. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0027] like Figure 1 As shown, a printing and dyeing method for alkali-soluble silk fabrics comprises the following steps:

[0028] S1: spinning the alkali-soluble silk fiber and the T400 fiber separately to obtain the alkali-soluble silk yarn and the T400 yarn.

[0029] S2: Weaving the alkali-soluble silk yarn and the T400 yarn, wherein both the warp yarn and the weft yarn contain the alkali-soluble silk yarn and the T400 yarn, to obtain an alkali-soluble silk coarse fabric.

[0030] S3: soaking the alkali-soluble silk coarse fabric in an alkali solution, dissolving the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric, taking out the alkali-soluble silk coarse fabric, washing and drying it.

[0031] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0032] The spinning treatment method of the alkali-soluble silk fiber in S1 is air-jet spinning or ring spinning, and the spinning treatment method of the T400 fiber is water-jet spinning. Air-jet spinning is a process that uses high-speed airflow to spin fibers. During the air-jet spinning process, the fibers are opened, stretched and spun into yarns, and the stretching is more uniform; ring spinning is a process that uses a ring-shaped spindle to spin fibers, which can produce yarns with higher strength and better wear resistance; during water-jet spinning, the fibers are subjected to less tensile force, which is conducive to maintaining the original properties of the fibers, such as strength and elasticity. Since the force applied during water-jet spinning is uniform and stable, the quality of the yarn produced is relatively stable. During water-jet spinning, only water power is needed to stretch the fibers into yarns, and no additional large amount of energy is consumed, which has significant energy-saving and environmental protection effects.

[0033] The raw materials of the alkali-soluble silk fiber in S1 include viscose fiber and flax fiber, and the viscose fiber and flax fiber exist in different fibers, respectively, to produce viscose yarn and flax yarn, respectively. Viscose fiber is a regenerated cellulose fiber, which is made by extracting cellulose from wood or cotton linters and then undergoing alkalization and dissolution. Due to its chemical modification, the crystallinity of viscose fiber is low and it is easier to dissolve in alkali solution; flax fiber is extracted from the stem of flax plant, which has high crystallinity and good stability. In alkali solution, flax fiber shows strong alkali resistance, only surface etching or slight degradation occurs, while the internal structure remains intact. When the yarn is prepared from viscose fiber and flax fiber respectively, the yarn made from viscose fiber is dissolved, and the yarn made from flax fiber is etched, which can present different forms of expression.

[0034] The fineness of viscose and flax in S1 is 1.2-1.8 dtex and 1.5-2.5 dtex respectively, and the fineness of T400 is 1.9-2.8 dtex. Viscose is a regenerated fiber, which is characterized by being easily dissolved under alkaline conditions. To achieve this goal, the fineness of the viscose yarn should be moderate, neither too thick to be difficult to dissolve nor too thin to affect the overall strength of the fabric. The fineness within this range ensures that the viscose fiber has enough reaction area in the alkali solution while maintaining the stability of the fabric. Flax is a natural fiber with high strength and wear resistance. In alkali solution, flax fibers will not be dissolved, but will be etched to a certain extent, resulting in a unique texture on the fiber surface. Within this range, sufficient fineness can ensure the strength and durability of the fiber. Since T400 yarn contains spandex, which has a strong tolerance to alkali, it is relatively stable in alkali solution. In order to ensure structural strength after the viscose yarn is dissolved, T400 yarn needs to have sufficient fineness and strength to withstand possible stress. The fineness in this range can ensure the stability of T400 yarn in alkali solution, while having sufficient strength and toughness to maintain the structural integrity of the fabric.

[0035] The number of viscose yarn and linen yarn in S1 is 20-30F and 60-80F respectively, and the number of T400 yarn is 100-140F. When the number of viscose yarn is 20-30F, it can maintain the balance in the weaving and dissolution process, and improve the dissolution rate of the alkaline solution while ensuring the successful manufacturing; when the number of linen yarn is 60-80F, it can improve the moisture absorption and air permeability of the fabric; in the process of alkali-soluble silk fabric soaking in alkaline solution, T400 yarn, as a stable fiber, can maintain the structure and shape of the fabric and ensure the air permeability of the fabric.

[0036] When weaving in S2, T400 yarn and linen yarn are arranged between adjacent viscose yarns in the warp yarn, the arrangement order of viscose yarn, T400 yarn and linen yarn is fixed, and the total number of T400 yarn and linen yarn between every two adjacent viscose yarns is the same. The arrangement order of viscose yarn, T400 yarn and linen yarn on the warp yarn is such that after being soaked in an alkaline solution, the basic structural strength of the fabric will not change, and the viscose yarn will not affect the overall structure of the fabric even after being dissolved.

[0037] When weaving in S2, the ratio of the number of T400 yarns between every two adjacent viscose yarns on the warp to the number of linen yarns is 1:1, and the T400 yarns and linen yarns between every two adjacent viscose yarns are arranged alternately, and the ratio of the number of viscose yarns to the number of linen yarns on the warp is 1:2-4. By arranging T400 yarns and linen yarns alternately in a ratio of 1:1, a balance of strength and elasticity can be achieved in the fabric, so that the fabric has good support and is soft and comfortable. The ratio of the number of viscose yarns to the number of linen yarns is 1:2-4, which ensures the number of micro-holes and micro-hole strips generated, so that the woven fabric has good air permeability.

[0038] When weaving in S2, the viscose yarn, linen yarn and T400 yarn in the weft yarn are arranged in a 1:1:1 interval order. By keeping the various yarns in the weft yarn arranged in a 1:1:1 interval order, the structure of the fabric can be ensured to be uniform, so that the texture and appearance of the fabric are more unified and coordinated; since the viscose yarn will be dissolved in the alkaline solution and the linen yarn will be etched, this uniform and orderly weaving method is conducive to the alkali dissolution process. The uniform distribution of viscose yarns ensures that the alkaline solution can penetrate into the fabric more effectively, thereby improving the efficiency of alkali dissolution and the uniformity of the final effect; since the viscose yarn will be dissolved in the alkaline solution and the linen yarn will be etched, this uniform and orderly weaving method is conducive to the alkali dissolution process. The uniform distribution of viscose yarns ensures that the alkaline solution can penetrate into the fabric more effectively, thereby improving the efficiency of alkali dissolution and the uniformity of the final effect.

[0039] The main component of the alkaline solution in S3 can be one or more of sodium hydroxide and sodium bicarbonate. Using these alkaline substances as the main components of the alkaline solution can ensure that the alkali-soluble silk yarn is effectively dissolved during the treatment process, thereby obtaining a fabric with the desired structure and characteristics. Using sodium hydroxide and / or sodium bicarbonate as the main components of the alkaline solution can more accurately control the alkali dissolution process. This precise control helps to improve the quality of the fabric.

[0040] The concentrations of sodium hydroxide and sodium bicarbonate in the alkaline solution in S3 are both 0.0001 mol / L, and the immersion time is 40-60 min. With a milder chemical force, this mild alkaline environment helps to ensure that the alkali-soluble silk yarn can be effectively dissolved, while reducing the potential damage to other yarns that are not involved in the alkali dissolution, and protecting the overall structure of the fabric. The combination of appropriate pH value and immersion time can improve the dissolution efficiency of alkali-soluble silk yarn. Within this pH range, the dissolution rate of viscose fiber is moderate, and it will not cause damage to the fabric structure due to too fast dissolution, nor will it affect production efficiency due to too slow dissolution.

[0041] The drying temperature in S3 is 90-120℃ and the drying time is 1h-2h. Drying at the appropriate temperature and time can help the fibers in the fabric to rearrange and fix, thereby stabilizing the structure of the fabric. This is very important for maintaining the dimensional stability and morphological integrity of the fabric. During the alkali dissolution process, the fabric may produce some internal stress. Through a proper drying process, these stresses can be effectively eliminated, reducing the internal damage of the fabric and improving the overall quality of the fabric.

[0042] The pH of the dyeing liquid in S4 should be maintained at 4-7.5. Keeping the pH value of the dyeing liquid within the range of 4-7.5 helps to protect the integrity of the fiber, ensure the quality and service life of the fabric, help improve the color fastness, ensure that the color after printing and dyeing is not easy to fade, and remain stable even under conditions such as sunlight, washing or friction, thus extending the service life of the fabric.

[0043] Embodiment 1

[0044] S1: 1.2 dtex viscose fiber, 2.0 dtex flax fiber and 2.8 dtex T400 fiber are ring-spun respectively to obtain 25F viscose yarn, 70F flax yarn and 120F T400 yarn.

[0045] S2: Weaving viscose yarn, linen yarn and T400 yarn, T400 yarn and linen yarn are arranged between adjacent viscose yarns in the warp yarn, the arrangement order of viscose yarn, T400 yarn and linen yarn is fixed, the ratio of the number of T400 yarns to the number of linen yarns between every two adjacent viscose yarns on the warp yarn is 1:1, the ratio of the number of viscose yarns to the number of linen yarns is 1:1, the T400 yarn and the linen yarn between every two adjacent viscose yarns are arranged alternately, and the viscose yarn, linen yarn and T400 yarn in the weft yarn are woven in sequence according to the order of 1:1:1 to obtain alkali-soluble silk coarse fabric.

[0046] S3: Soak the alkali-soluble silk coarse fabric in an alkaline solution with a sodium hydroxide and sodium bicarbonate concentration of 0.0001 mol / L for 50 minutes, and the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric is dissolved. The alkali-soluble silk coarse fabric is taken out, washed and dried at a drying temperature of 100°C and a drying time of 1 hour.

[0047] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0048] Embodiment 2

[0049] S1: 1.2 dtex viscose fiber, 2.0 dtex flax fiber and 2.8 dtex T400 fiber are ring-spun respectively to obtain 25F viscose yarn, 70F flax yarn and 120F T400 yarn.

[0050] S2: Weaving viscose yarn, linen yarn and T400 yarn, T400 yarn and linen yarn are arranged between adjacent viscose yarns in the warp yarn, the arrangement order of viscose yarn, T400 yarn and linen yarn is fixed, the ratio of the number of T400 yarns to the number of linen yarns between every two adjacent viscose yarns on the warp yarn is 1:1, the ratio of the number of viscose yarns to the number of linen yarns is 1:2, the T400 yarn and the linen yarn between every two adjacent viscose yarns are arranged alternately, and the viscose yarn, linen yarn and T400 yarn in the weft yarn are woven in sequence according to the order of 1:1:1 to obtain alkali-soluble silk coarse fabric.

[0051] S3: Soak the alkali-soluble silk coarse fabric in an alkaline solution with a sodium hydroxide and sodium bicarbonate concentration of 0.0001 mol / L for 50 minutes, and the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric is dissolved. The alkali-soluble silk coarse fabric is taken out, washed and dried at a drying temperature of 100°C and a drying time of 1 hour.

[0052] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0053] Embodiment 3

[0054] S1: 1.2 dtex viscose fiber, 2.0 dtex flax fiber and 2.8 dtex T400 fiber are ring-spun respectively to obtain 25F viscose yarn, 70F flax yarn and 120F T400 yarn.

[0055] S2: Weaving viscose yarn, linen yarn and T400 yarn, T400 yarn and linen yarn are arranged between adjacent viscose yarns in the warp yarn, the arrangement order of viscose yarn, T400 yarn and linen yarn is fixed, the ratio of the number of T400 yarns to the number of linen yarns between every two adjacent viscose yarns on the warp yarn is 1:1, the ratio of the number of viscose yarns to the number of linen yarns is 1:3, the T400 yarn and the linen yarn between every two adjacent viscose yarns are arranged alternately, and the viscose yarn, linen yarn and T400 yarn in the weft yarn are woven in sequence according to the order of 1:1:1 to obtain alkali-soluble silk coarse fabric.

[0056] S3: Soak the alkali-soluble silk coarse fabric in an alkaline solution with a sodium hydroxide and sodium bicarbonate concentration of 0.0001 mol / L for 50 minutes, and the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric is dissolved. The alkali-soluble silk coarse fabric is taken out, washed and dried at a drying temperature of 100°C and a drying time of 1 hour.

[0057] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0058] Embodiment 4

[0059] S1: 1.2 dtex viscose fiber, 2.0 dtex flax fiber and 2.8 dtex T400 fiber are ring-spun respectively to obtain 25F viscose yarn, 70F flax yarn and 120F T400 yarn.

[0060] S2: Weaving viscose yarn, linen yarn and T400 yarn, T400 yarn and linen yarn are arranged between adjacent viscose yarns in the warp yarn, the arrangement order of viscose yarn, T400 yarn and linen yarn is fixed, the ratio of the number of T400 yarns to the number of linen yarns between every two adjacent viscose yarns on the warp yarn is 1:1, the ratio of the number of viscose yarns to the number of linen yarns is 1:4, the T400 yarn and the linen yarn between every two adjacent viscose yarns are arranged alternately, and the viscose yarn, linen yarn and T400 yarn in the weft yarn are woven in sequence according to the order of 1:1:1 to obtain alkali-soluble silk coarse fabric.

[0061] S3: Soak the alkali-soluble silk coarse fabric in an alkaline solution with a sodium hydroxide and sodium bicarbonate concentration of 0.0001 mol / L for 50 minutes, and the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric is dissolved. The alkali-soluble silk coarse fabric is taken out, washed and dried at a drying temperature of 100°C and a drying time of 1 hour.

[0062] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0063] Embodiment 5

[0064] S1: 1.2 dtex viscose fiber, 2.0 dtex flax fiber and 2.8 dtex T400 fiber are ring-spun respectively to obtain 25F viscose yarn, 70F flax yarn and 120F T400 yarn.

[0065] S2: Weaving viscose yarn, linen yarn and T400 yarn, T400 yarn and linen yarn are arranged between adjacent viscose yarns in the warp yarn, the arrangement order of viscose yarn, T400 yarn and linen yarn is fixed, the ratio of the number of T400 yarns to the number of linen yarns between every two adjacent viscose yarns on the warp yarn is 1:1, the ratio of the number of viscose yarns to the number of linen yarns is 1:5, the T400 yarn and the linen yarn between every two adjacent viscose yarns are arranged alternately, and the viscose yarn, linen yarn and T400 yarn in the weft yarn are woven in sequence according to the order of 1:1:1 to obtain alkali-soluble silk coarse fabric.

[0066] S3: Soak the alkali-soluble silk coarse fabric in an alkaline solution with a sodium hydroxide and sodium bicarbonate concentration of 0.0001 mol / L for 50 minutes, and the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric is dissolved. The alkali-soluble silk coarse fabric is taken out, washed and dried at a drying temperature of 100°C and a drying time of 1 hour.

[0067] S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

[0068] The samples of Examples 1 to 5, each with a length of 10 cm, were tested according to GB / T5453-1997 Determination of Air Permeability of Textile Fabrics. The test results are shown in Table 1.

[0069] Table 1 Air permeability test results in Examples 1 to 5

[0070] sample Air permeability (mm / s) Embodiment 1 1402.4 Embodiment 2 1437.9 Embodiment 3 1456.7 Embodiment 4 1440.3 Embodiment 5 1409.6

[0071] It can be seen from Table 1 that in Examples 1 to 5, the air permeability first increases and then decreases, because the ratio of the number of linen yarn and T400 yarn in the yarn gradually increases, which increases the number of micro-holes and micro-void strips on the T400 yarn. However, as the ratio gradually increases, the tightness between the linen yarn and the T400 yarn increases, reducing the air permeability of the fabric.

[0072] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.

Claims

1. A printing and dyeing method for alkali-soluble silk fabrics, characterized in that: The following steps are involved: S1: spinning the alkali-soluble silk fiber and the T400 fiber separately to obtain the alkali-soluble silk yarn and the T400 yarn; S2: weaving the alkali-soluble silk yarn and the T400 yarn, wherein both the warp yarn and the weft yarn contain the alkali-soluble silk yarn and the T400 yarn, to obtain an alkali-soluble silk coarse fabric; S3: soaking the alkali-soluble silk coarse fabric in an alkali solution, dissolving the alkali-soluble silk yarn on the alkali-soluble silk coarse fabric, taking out the alkali-soluble silk coarse fabric, washing and drying; S4: printing and dyeing the alkali-soluble silk coarse fabric to obtain the alkali-soluble silk fabric.

2. A printing and dyeing method for alkali-soluble silk fabric according to claim 1, characterized in that: The spinning treatment method of the alkali-soluble silk fiber in S1 is one of air-jet spinning and ring spinning, and the spinning treatment method of the T400 fiber is water-jet spinning.

3. A printing and dyeing method for alkali-soluble silk fabric according to claim 1, characterized in that: The raw materials of the alkali-soluble silk fiber in S1 include viscose fiber and flax fiber, and the viscose fiber and flax fiber exist in different fibers respectively, and viscose yarn and flax yarn are prepared respectively.

4. A printing and dyeing method for alkali-soluble silk fabric according to claim 3, characterized in that: The fineness of the viscose fiber and the flax fiber in S1 is 1.2-1.8 dtex and 1.5-2.5 dtex respectively, and the fineness of the T400 fiber is 1.9-2.8 dtex.

5. A printing and dyeing method for alkali-soluble silk fabric according to claim 3, characterized in that: During weaving in S2, T400 yarns and linen yarns are arranged between adjacent viscose yarns in the warp yarns, the arrangement order of the viscose yarns, T400 yarns and linen yarns is fixed, and the total number of T400 yarns and linen yarns between every two adjacent viscose yarns is the same.

6. A printing and dyeing method for alkali-soluble silk fabric according to claim 5, characterized in that: During weaving in S2, the ratio of the number of T400 yarns between every two adjacent viscose yarns on the warp to the number of linen yarns is 1:1, and the T400 yarns and linen yarns between every two adjacent viscose yarns are arranged alternately, and the ratio of the number of viscose yarns to the number of linen yarns on the warp is 1:2-4.

7. A printing and dyeing method for alkali-soluble silk fabric according to claim 3, characterized in that: During weaving in S2, the viscose yarn, the linen yarn and the T400 yarn in the weft yarn are arranged in a 1:1:1 interval sequence.

8. A printing and dyeing method for alkali-soluble silk fabric according to claim 1, characterized in that: The main component of the alkaline solution in S3 can be one or more of sodium hydroxide and sodium bicarbonate.

9. A printing and dyeing method for alkali-soluble silk fabric according to claim 1, characterized in that: The concentrations of sodium hydroxide and sodium bicarbonate in the alkaline solution in S3 are both 0.0001 mol / L, and the soaking time is 40 min-60 min.

10. A printing and dyeing method for alkali-soluble silk fabric according to claim 1, characterized in that: The drying temperature in S3 is 90-120° C., and the drying time is 1 h-2 h.