Method for measuring content of silicon dioxide in glass peening shot
By mixing and melting glass shot peening with a strong alkali and measuring it using inductively coupled plasma spectrometry, the problem of low accuracy and safety hazards in the existing glass shot peening silica content determination methods has been solved, and rapid and accurate measurement has been achieved. Silica content detection.
Patent Information
- Application Number
- CN202410899953.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
AI Technical Summary
The existing methods for measuring silica content in glass shot peening have problems such as long test cycles, low accuracy and potential safety hazards.
The glass to be tested is shot peened and solid strong alkali is mixed evenly and then melted, then the leachate and acidic solution are added for dissolution, and then the silica content is determined by inductively coupled plasma spectrometry, and hydrochloric acid and nitric acid are used to adjust the acidity of the system to avoid Complex sample processing procedures and high-temperature heating improve the safety and accuracy of the test.
It simplifies the dissolution process of glass shot peening, improves the accuracy of measuring silica content, shortens detection time, reduces experimental risks, and is suitable for accurate detection of a variety of glass beads.
Smart Images

Figure CN118777008A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aviation parts and supporting products, and relates to a method for determining the content of silicon dioxide in glass shot peening. Background Art
[0002] Shot peening technology is widely used in the aviation field for surface strengthening of parts. Aircraft engines are the power components of aircraft. They are in high-speed, high-pressure and high-intensity operation states, and the performance requirements of engine parts are extremely strict. Engine parts work under alternating loads, and the fatigue life of parts is very high. Shot peening is an effective method to improve the fatigue life of parts. Generally, the fatigue life of parts treated with shot peening is increased by 1 to several times compared with those without shot peening. The principle of shot peening is that the high-speed projectile flow continuously impacts the surface of the metal material, causing the metal surface layer to produce extremely strong plastic deformation. The depth of this plastic deformation layer is usually 0.1 to 0.8 mm, and a residual stress field is formed on the surface of the material, and the surface roughness and surface morphology also change. Roughness can be changed by secondary shot peening or surface finishing. Various changes on the surface of the material will significantly improve the material's fatigue resistance and stress corrosion resistance, so that the material surface can be strengthened. The silica content in the glass shot in the shot peening process seriously affects the strengthening efficiency and surface quality of the glass shot, so the determination of its content requirements is crucial.
[0003] At present, the chemical analysis methods that can be used for reference at home and abroad include GB / T1347-2008 "Chemical Analysis Methods for Soda-lime-silica Glass". This method uses potassium silicofluoride volumetric method to determine silicon dioxide. After the sample is dissolved in nitric acid and hydrofluoric acid, potassium nitrate is added to make silicon generate potassium silicofluoride precipitation. After the precipitation is filtered and dissolved with hot water, the hydrofluoric acid quantitatively precipitated by potassium silicofluoride is titrated with sodium hydroxide standard solution, and the percentage of silicon is calculated. During the test, high-temperature heating is required in stages. On the one hand, there are high-temperature safety hazards. On the other hand, manual supervision is required, which increases the test cost. In addition, multiple filtration and washing are required, resulting in sample loss. The test results are not accurate, the titration process is not easy to control, and the operator's ability requirements are high. The test results are greatly affected by human interference. In addition, the experimental process involves the use of hydrofluoric acid, which has safety hazards and the test process is also long. GB / T6900~2016 "Chemical Analysis Methods of Aluminum Silicon Refractories" uses molybdenum blue spectrophotometry to determine silicon dioxide. This method is often used to detect samples with a silicon dioxide content of no more than 5%. When used for high-content silicon dioxide determination, the detection range is not applicable. ASTM C169 "Standard Test Methods for Chemical Analysis of Soda~Lime and Borosilicate Glass" uses a gravimetric method combined with molybdenum blue spectrophotometry to determine silicon dioxide content. During the determination process, both the precipitate and the filtrate contain silicon. The silicon in the precipitate is determined by gravimetric method, which involves high-temperature burning, the use of hydrofluoric acid and multiple weighing. The silicon in the filtrate is determined by molybdenum blue spectrophotometry. The entire determination process is complicated, the determination cycle is too long, and the accuracy is low. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a method for determining the silicon dioxide content in glass shot, thereby solving the technical problems of the existing testing method, such as long testing cycle, low accuracy of test results and potential safety hazards in the testing process.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for determining the content of silicon dioxide in glass shot peening comprises the following steps:
[0007] S1: Evenly mix the glass shot to be tested with a solid strong base, melt the mixture, add a leaching solution to the obtained melt to obtain a mixed system, boil the mixed system, and then add hydrochloric acid and nitric acid until the leached melt is completely dissolved to obtain a solution to be tested;
[0008] S2: Using inductively coupled plasma spectrometry and a preset standard curve to determine the content of silicon dioxide in the glass shot to be tested.
[0009] Preferably, in step S1, the mass ratio of the glass shot to be tested to the solid strong alkali is 1:(15-20).
[0010] Preferably, in step S1, the strong base is sodium hydroxide or potassium hydroxide.
[0011] Preferably, in step S1, the temperature of the melting process is 370-410°C.
[0012] Preferably, in step S1, the extracting solution is boiling water.
[0013] Preferably, in step S1, after boiling the mixed system, keep it for 3 to 5 minutes, cool it to 10 to 25° C., and then add hydrochloric acid and nitric acid.
[0014] Preferably, in step S1, the ratio of the glass shot to be tested to hydrochloric acid and nitric acid is 0.1 g: (45-55) mL: (3-8) mL.
[0015] Preferably, the mass concentration of the hydrochloric acid is 0.5-1 g / mL, and the mass concentration of the nitric acid is 1-2 g / mL.
[0016] Preferably, in step S2, when the inductively coupled plasma spectrometry method is used for testing, the testing is performed at a wavelength of 251 nm.
[0017] Preferably, in step S2, the content of silicon dioxide in the glass shot to be tested is:
[0018]
[0019] In the formula,
[0020] ρ M is the mass concentration of silicon dioxide in the test solution in step S1 determined by the standard curve;
[0021] ρ0 is the mass concentration of silica in the blank solution;
[0022] V is the volume of the solution to be tested in step S1;
[0023] m is the mass of the glass shot to be tested.
[0024] Compared with the prior art, the present invention has the following beneficial technical effects:
[0025] The present invention discloses a method for determining the content of silicon dioxide in glass shot. The method mainly includes dissolving and analyzing the sample to be tested. In the dissolving process of the sample to be tested, the glass shot to be tested is firstly mixed with a solid strong alkali and melted. During the melting process, the silicon dioxide reacts with the strong alkali to obtain silicate, and then an extract is added and boiled to fully dissolve the silicate in the extract. Finally, hydrochloric acid and nitric acid are used to treat the system. On the one hand, the metal oxide or impurities introduced into the system in the above steps can be dissolved, and on the other hand, it can be used to adjust the acidity of the system for subsequent testing. Using other common acids, such as sulfuric acid, will cause the system to be dehydrated, and the dissolved silicon will re-condense and precipitate, resulting in a large test error. In addition, sulfuric acid will also damage the fine parts of the test equipment, affect the atomization injection amount of the pneumatic atomizer and the size of the aerosol particles, and then affect the spectral line intensity. In addition, sulfuric acid, as a strong acid, will produce strong background absorption, making it difficult to accurately distinguish the signal of the element to be tested in the spectrum test. In addition, this background absorption will interfere with the signal of silicon and affect the accuracy of the measurement result. Therefore, hydrochloric acid with little background interference and no damage to the equipment is used to effectively ensure the accuracy of the test while achieving rapid dissolution of the sample. Finally, the inductively coupled plasma spectrometry method is used to determine the silica content in the glass shot. This method uses a strong alkali to melt the glass shot to be tested, and then uses an extract to extract the test object. The impurities in the system are dissolved by hydrochloric acid and nitric acid, and the acidity value of the system is adjusted to achieve effective dissolution of silica in the glass shot to be tested. During the dissolution process, the processing steps of the glass shot to be tested are reduced, the dissolution process of the glass shot to be tested is simplified, and the sample loss caused by the complex sample processing process is avoided, thereby improving the accuracy of the test, shortening the detection time, and improving the safety of the test.
[0026] Furthermore, in step S1, the mass ratio of the glass shot to be tested to the solid strong base is 1:(15-20). The higher solid strong base ratio ensures that the glass shot can fully react with the strong base during the melting process, thereby more completely converting into a melt soluble in acid, which is helpful for the extraction and determination of silicon dioxide in the subsequent steps. Since the melting process is more complete and the interference of impurities is reduced, the silicon dioxide content subsequently determined by inductively coupled plasma spectrometry will be more accurate.
[0027] Furthermore, in step S1, the strong base is sodium hydroxide or potassium hydroxide, both of which are strong bases with high alkalinity and strong reactivity, which ensures that they can fully react with the glass shot to be tested during the melting process and convert it into a melt soluble in acid.
[0028] Furthermore, in step S1, the temperature of the melting process is 370-410°C. Within this temperature range, the glass shot and the solid strong alkali can fully react and completely melt. This helps to convert the silicate components in the glass shot into silicate, providing accurate samples for subsequent analysis steps. At the same time, the appropriate temperature can accelerate the rate of chemical reactions. Within this temperature range, the melting process can proceed rapidly, reducing the experimental time and improving the analysis efficiency.
[0029] Furthermore, in step S1, the leaching solution is boiling water. The high temperature of boiling water helps to promote the dissolution and leaching of silicate components in the melt. The high temperature can accelerate the thermal motion of molecules, making it easier for ions and molecules in the solution to contact and react with silicate components in the melt, thereby improving the leaching efficiency. Boiling water, as a relatively pure solvent, reduces impurities that may be introduced by other solvents. This helps to maintain the purity of the solution to be tested and improve the accuracy of the analysis. Using boiling water as a leaching solution is simple to operate, and does not require the use of other special solvents or equipment. It is safer and reduces the risk of experimental operations.
[0030] Further, in step S1, after boiling the mixed system, keep it for 3 to 5 minutes, cool it to 10 to 25°C, and then add hydrochloric acid and nitric acid. Boiling the mixed system helps to further promote the reaction between the silicate components in the melt and the leaching solution, ensuring that the reaction is more complete. The process of cooling to 10 to 25°C after boiling helps to control the temperature when hydrochloric acid and nitric acid are subsequently added. The appropriate temperature range can ensure that hydrochloric acid and nitric acid fully react with other metal impurities in the system, while avoiding side reactions or safety risks caused by excessively high temperatures. Adding hydrochloric acid and nitric acid at a lower temperature can optimize the reaction conditions and make the reaction more stable and controllable. This helps to reduce experimental errors and improve the accuracy of analytical results.
[0031] Furthermore, in step S1, the ratio of the glass shot to be tested to hydrochloric acid and nitric acid is 0.1 g: (45-55) mL: (3-8) mL, which ensures that the metal impurities or metal oxide impurities in the system are fully dissolved, reduces their interference with the determination of silicon dioxide content, and improves the accuracy of the test results.
[0032] Furthermore, the mass concentration of the hydrochloric acid is 0.5-1 g / mL, and the mass concentration of the nitric acid is 1-2 g / mL, which ensures the full dissolution of the corresponding impurities, while making the system acidity adjustment process faster and shortening the sample processing cycle.
[0033] Further, when the inductively coupled plasma spectrometry is used for testing in step S2, the test is performed at a wavelength of 251nm. At 251nm, the element to be tested can produce a strong characteristic spectrum, thereby achieving high-sensitivity detection of the element to be tested, which helps to obtain more accurate and reliable test results. When the test is performed at a wavelength of 251nm, since the spectral signal is strong, the analysis time can be further shortened and the test efficiency can be improved. When the test is performed at a wavelength of 251nm, since the signal intensity is high, the detection limit may be further reduced, thereby achieving accurate detection of trace elements. When the test is performed at a wavelength of 251nm, since the spectral signal has a strong specificity, the interference of other elements can be effectively reduced, and the accuracy of the test can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0035] Figure 1 It is a schematic flow chart of a method for determining the content of silicon dioxide in glass shot peening in the present invention;
[0036] Figure 2 This is the standard curve established in Example 1 of the present invention. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0038] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0039] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0040] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0041] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0042] like Figure 1 As shown, the present invention provides a method for determining the content of silicon dioxide in glass shot, comprising the following steps:
[0043] S1: Evenly mix the glass shot to be tested with the solid strong base, melt the mixture at 370-410°C, add the leaching solution to the obtained melt to obtain a mixed system, boil the mixed system, keep it for 3-5 minutes, cool it to 10-25°C, and then add hydrochloric acid and nitric acid until the leached melt is completely dissolved to obtain a solution to be tested;
[0044] The mass ratio of the glass shot to be tested to the solid strong base is 1:(15-20). The strong base is sodium hydroxide or potassium hydroxide. The leaching solution is boiling water. The ratio of the glass shot to be tested to hydrochloric acid and nitric acid is 0.1g:(45-55)mL:(3-8)mL. The mass concentration of hydrochloric acid is 0.5-1g / mL, and the mass concentration of nitric acid is 1-2g / mL.
[0045] S2: Using inductively coupled plasma spectrometry and a preset standard curve, determine the content of silicon dioxide in the glass shot to be tested. When using inductively coupled plasma spectrometry, the test is performed at a wavelength of 251 nm. At the same time, each sample is tested three times, and the average value of the test results is taken as the final result.
[0046] The content of silicon dioxide in the glass shot to be tested is:
[0047]
[0048] In the formula,
[0049] ρ M is the mass concentration of silicon dioxide in the test solution in step S1 determined by the standard curve;
[0050] ρ0 is the mass concentration of silica in the blank solution;
[0051] V is the volume of the solution to be tested in step S1;
[0052] m is the mass of the glass shot to be tested.
[0053] The principle of this method is to melt with a strong alkali, then leaching with boiling water, and using an inductively coupled plasma analyzer to measure the spectral intensity value of silicon in the solution to calculate the content of silicon dioxide. This method uses a strong alkali for melting, which can completely melt the sample, avoiding the operational risks of medium and high temperature segmented melting, and the melting process does not require manual supervision. The leaching process is simple, reducing the loss of samples during the test. Hydrofluoric acid is not used in the test process to avoid safety risks. This method prepares the sample once, without the need for multiple weighing and heating, and can directly analyze the silicon element with high accuracy, which can achieve the purpose of accurate analysis. This method is quick and simple, uses simple and commonly used reagents, has a short analysis cycle, saves costs, and improves work efficiency by 60%. It is suitable for accurate detection of silicon elements and their compounds in glass beads with a diameter of 10 microns (BZ10), or BZ15, BZ20, BZ25, BZ35, and BZ50.
[0054] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only intended to clarify the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0055] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0056] Example 1
[0057] A method for determining the content of silicon dioxide in glass shot is achieved by the following steps:
[0058] (1) Preparation of sample solution: according to the silicon content range in the sample, weigh 0.1 g of the sample into an iron / nickel crucible, add 2 g of sodium hydroxide, mix well, and melt in a muffle furnace at 400°C for 1 h. After cooling, use hot water to immerse the melt into a 500 mL polytetrafluoroethylene beaker, then wash the crucible with a small amount of hydrochloric acid and water, and put the washing liquid into the beaker. Control the volume of the test solution to about 100 mL, boil for 3 min, cool slightly, add 50 mL of hydrochloric acid and 5 mL of nitric acid, dissolve at low temperature until clear, remove and cool, transfer to a 500 mL volumetric flask, dilute to the mark, and shake well to obtain test solution A;
[0059] (2) Prepare a blank solution simultaneously: all steps are the same as (1) except that no sample is added;
[0060] (3) Preparation of standard solution: Weigh 3 parts of silicon dioxide equivalent to the lower limit, middle limit, and upper limit of the content in the sample, add 2 g of sodium hydroxide, calcine at 400°C for 1 h, soak and place in a 500 mL volumetric flask, cool slightly and then dilute to the mark to obtain a standard solution.
[0061] (4) Draw the working curve: Select silicon element, wavelength 251nm. Perform blank measurement successively, and measure the standard solution from low to high silicon content. Obtain the silicon content working curve of the inductively coupled plasma spectrometer, as shown in Figure 2 As shown, the contents of silicon dioxide in the standard solutions are 72%, 70.4% and 67.2%, respectively, and the corresponding intensities are 81452.27, 79578.71 and 76022.12, respectively.
[0062] (5) Measurement: Take 10 mL of test solution A in a 100 mL volumetric flask, dilute to the mark, shake well, and introduce into the inductively coupled plasma spectrometer to measure silicon. The concentration of silicon dioxide in the tested solution can be obtained according to the peak curve of the excitation, or the corresponding silicon dioxide content can be directly given.
[0063] (6) Calculation of silicon dioxide content:
[0064]
[0065] In the formula
[0066] ρ M The mass concentration of silicon in the test solution A in step (1) is obtained from the working curve, i.e., the standard curve, in micrograms per milliliter (μg / mL);
[0067] ρ0 is the mass concentration of silicon in the blank solution obtained from the working curve, in micrograms per milliliter (μg / mL);
[0068] V is the volume of test solution A in step (1), in milliliters (mL);
[0069] m is the mass of the sample in step (1), in g (g).
[0070] Example 2
[0071] A method for determining the content of silicon dioxide in glass shot peening comprises the following steps:
[0072] Step 1: Weighing of sample: Weigh 0.1g BZ15 sample into an iron / nickel crucible, add 1.5g sodium hydroxide and mix well.
[0073] Step 2: Melting of the sample: Melt in a muffle furnace at 370°C for 1 hour, then take out and cool.
[0074] Step 3: Preparation of test solution. Use hot water to soak the melt in a 500mL polytetrafluoroethylene beaker, then use a small amount of hydrochloric acid and water to clean the crucible, add the washing liquid to the beaker, control the volume of the test solution to about 100mL, boil for 3-5min, cool slightly, add 50mL of 1:1 hydrochloric acid and 5mL of nitric acid, dissolve at low temperature until clear, remove and cool, transfer to a 500mL volumetric flask, dilute to the mark, shake well, and obtain test solution A;
[0075] Step 4: Prepare a blank solution: except that no sample is added, all other steps are the same as 1 to 3;
[0076] Step 5: Prepare standard solution: weigh 3 parts of silicon dioxide equivalent to the lower limit, medium limit and upper limit of the content in the sample respectively, add 1.5g of sodium hydroxide, calcine at 370℃ for 1h, soak and place in a 500mL volumetric flask, cool slightly and then dilute to the scale to obtain a standard solution.
[0077] Step 6: Draw the working curve: Select silicon element, wavelength 251nm. Perform blank measurement, and measure the standard solution from low to high silicon content. Obtain the silicon content working curve of the inductively coupled plasma spectrometer.
[0078] Step 7: Take 10 mL of test solution A and put it into a 100 mL volumetric flask, dilute to the mark, shake well, and introduce it into the inductively coupled plasma spectrometer to determine the silicon content.
[0079] Step 8: Calculate according to the formula:
[0080] Example 3
[0081] A method for determining the content of silicon dioxide in glass shot peening comprises the following steps:
[0082] Step 1: Weighing of sample: Weigh 0.1g BZ15 sample into an iron / nickel crucible, add 2.0g sodium hydroxide and mix well.
[0083] Step 2: Melting of the sample: Melt in a muffle furnace at 410°C for 1 hour, then take out and cool.
[0084] Step 3: Preparation of test solution. Use hot water to soak the melt in a 500mL polytetrafluoroethylene beaker, then use a small amount of hydrochloric acid and water to clean the crucible, add the washing liquid to the beaker, control the volume of the test solution to about 100mL, boil for 3-5min, cool slightly, add 50mL of 1:1 hydrochloric acid and 5mL of nitric acid, dissolve at low temperature until clear, remove and cool, transfer to a 500mL volumetric flask, dilute to the mark, shake well, and obtain test solution A;
[0085] Step 4: Prepare a blank solution: except that no sample is added, all other steps are the same as 1 to 3;
[0086] Step 5: Prepare standard solution: weigh 3 parts of silicon dioxide equivalent to the lower limit, medium limit and upper limit of the content in the sample respectively, add 2.0g of sodium hydroxide, calcine at 410℃ for 1h, soak and place in a 500mL volumetric flask, cool slightly and then dilute to the scale to obtain a standard solution.
[0087] Step 6: Draw the working curve: Select silicon element, wavelength 251nm. Perform blank measurement, and measure the standard solution from low to high silicon content. Obtain the silicon content working curve of the inductively coupled plasma spectrometer.
[0088] Step 7: Take 10 mL of test solution A and put it into a 100 mL volumetric flask, dilute to the mark, shake well, and introduce it into the inductively coupled plasma spectrometer to determine the silicon content.
[0089] Step 8: Calculate according to the formula:
[0090] Example 4
[0091] A method for determining the content of silicon dioxide in glass shot peening comprises the following steps:
[0092] Step 1: Weighing of sample: Weigh 0.1g BZ25 sample into an iron / nickel crucible, add 3.0g sodium hydroxide and mix well.
[0093] Step 2: Melting of the sample: Melt in a muffle furnace at 410°C for 1 hour, then take out and cool.
[0094] Step 3: Preparation of test solution. Use hot water to soak the melt in a 500mL polytetrafluoroethylene beaker, then use a small amount of hydrochloric acid and water to clean the crucible, add the washing liquid to the beaker, control the volume of the test solution to about 100mL, boil for 3-5min, cool slightly, add 50mL of 1:1 hydrochloric acid and 5mL of nitric acid, dissolve at low temperature until clear, remove and cool, transfer to a 500mL volumetric flask, dilute to the mark, shake well, and obtain test solution A;
[0095] Step 4: Prepare a blank solution: All steps are the same as 1 to 3 except that no sample solution is added;
[0096] Step 5: Prepare standard solution: weigh 3 parts of silicon dioxide equivalent to the lower limit, medium limit and upper limit of the content in the sample respectively, add 3.0g of sodium hydroxide, calcine at 410℃ for 1h, soak and place in a 500mL volumetric flask, cool slightly and then dilute to the scale to obtain a standard solution.
[0097] Step 6: Draw the working curve: Select silicon element, wavelength 251nm. Perform blank measurement, and measure the standard solution from low to high silicon content. Obtain the silicon content working curve of the inductively coupled plasma spectrometer.
[0098] Step 7: Take 10 mL of test solution A and put it into a 100 mL volumetric flask, dilute to the mark, shake well, and introduce it into the inductively coupled plasma spectrometer to determine the silicon content.
[0099] Step 8: Calculate according to the formula:
[0100] Example 5
[0101] A method for determining the content of silicon dioxide in glass shot peening comprises the following steps:
[0102] Step 1: Weighing of sample: Weigh 0.1g BZ25 sample into an iron / nickel crucible, add 2.5g sodium hydroxide and mix well.
[0103] Step 2: Melting of the sample: Melt in a muffle furnace at 390°C for 1 hour, then take out and cool.
[0104] Step 3: Preparation of test solution. Use hot water to soak the melt in a 500mL polytetrafluoroethylene beaker, then use a small amount of hydrochloric acid and water to clean the crucible, add the washing liquid to the beaker, control the volume of the test solution to about 100mL, boil for 3-5min, cool slightly, add 50mL of 1:1 hydrochloric acid and 5mL of nitric acid, dissolve at low temperature until clear, remove and cool, transfer to a 500mL volumetric flask, dilute to the mark, shake well, and obtain test solution A;
[0105] Step 4: Prepare a blank solution: All steps are the same as 1 to 3 except that no sample solution is added;
[0106] Step 5: Prepare standard solution: weigh 3 parts of silicon dioxide equivalent to the lower limit, medium limit and upper limit of the content in the sample respectively, add 2.5g of sodium hydroxide, calcine at 390℃ for 1h, soak and place in a 500mL volumetric flask, cool slightly and then dilute to the scale to obtain a standard solution.
[0107] Step 6: Draw the working curve: Select silicon element, wavelength 251nm. Perform blank measurement, and measure the standard solution from low to high silicon content. Obtain the silicon content working curve of the inductively coupled plasma spectrometer.
[0108] Step 7: Take 10 mL of test solution A and put it into a 100 mL volumetric flask, dilute to the mark, shake well, and introduce it into the inductively coupled plasma spectrometer to determine the silicon content.
[0109] Step 8: Calculate according to the formula:
[0110] Example 6
[0111] A method for determining the content of silicon dioxide in glass shot peening comprises the following steps:
[0112] Step 1: Weighing of sample: Weigh 0.1g BZ25 sample into an iron / nickel crucible, add 2.0g potassium hydroxide and mix well.
[0113] Step 2: Melting of the sample: Melt in a muffle furnace at 410°C for 1 hour, then take out and cool.
[0114] Step 3: Preparation of test solution. Use hot water to soak the melt in a 500mL polytetrafluoroethylene beaker, then use a small amount of hydrochloric acid and water to clean the crucible, add the washing liquid to the beaker, control the volume of the test solution to about 100mL, boil for 3-5min, cool slightly, add 50mL of 1:1 hydrochloric acid and 5mL of nitric acid, dissolve at low temperature until clear, remove and cool, transfer to a 500mL volumetric flask, dilute to the mark, shake well, and obtain test solution A;
[0115] Step 4: Prepare a blank solution: All steps are the same as 1 to 3 except that no sample solution is added;
[0116] Step 5: Prepare standard solution: weigh 3 parts of silicon dioxide equivalent to the lower limit, medium limit and upper limit of the content in the sample respectively, add 2.0g of sodium hydroxide, calcine at 410℃ for 1h, soak and place in a 500mL volumetric flask, cool slightly and then dilute to the scale to obtain a standard solution.
[0117] Step 6: Draw the working curve: Select silicon element, wavelength 251nm. Perform blank measurement, and measure the standard solution from low to high silicon content. Obtain the silicon content working curve of the inductively coupled plasma spectrometer.
[0118] Step 7: Take 10 mL of test solution A and put it into a 100 mL volumetric flask, dilute to the mark, shake well, and introduce it into the inductively coupled plasma spectrometer to determine the silicon content.
[0119] Step 8: Calculate according to the formula:
[0120] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for determining the content of silicon dioxide in glass shot, characterized in that: The following steps are involved: S1: Evenly mix the glass shot to be tested with a solid strong base, melt the mixture, add a leaching solution to the obtained melt to obtain a mixed system, boil the mixed system, and then add hydrochloric acid and nitric acid until the leached melt is completely dissolved to obtain a solution to be tested; S2: Using inductively coupled plasma spectrometry and a preset standard curve to determine the content of silicon dioxide in the glass shot to be tested.
2. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S1, the mass ratio of the glass shot to be tested to the solid strong alkali is 1:(15-20).
3. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S1, the strong base is sodium hydroxide or potassium hydroxide.
4. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S1, the temperature of the melting process is 370-410°C.
5. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S1, the extracting liquid is boiling water.
6. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S1, the mixed system is boiled and kept for 3 to 5 minutes, cooled to 10 to 25° C., and then hydrochloric acid and nitric acid are added.
7. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S1, the ratio of the glass shot to be tested to hydrochloric acid and nitric acid is 0.1 g: (45-55) mL: (3-8) mL.
8. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: The mass concentration of the hydrochloric acid is 0.5-1 g / mL, and the mass concentration of the nitric acid is 1-2 g / mL.
9. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S2, when the inductively coupled plasma spectrometry method is used for testing, the testing is performed at a wavelength of 251 nm.
10. The method for determining the content of silicon dioxide in glass shot according to claim 1, characterized in that: In step S2, the content of silicon dioxide in the glass shot to be tested is: In the formula, ρ M is the mass concentration of silicon dioxide in the test solution in step S1 determined by the standard curve; ρ0 is the mass concentration of silica in the blank solution; V is the volume of the solution to be tested in step S1; m is the mass of the glass shot to be tested.